<?xml-model href='http://www.tei-c.org/release/xml/tei/custom/schema/relaxng/tei_all.rng' schematypens='http://relaxng.org/ns/structure/1.0'?><TEI xmlns="http://www.tei-c.org/ns/1.0">
	<teiHeader>
		<fileDesc>
			<titleStmt><title level='a'>Magnetoelectric Coupling by Piezoelectric Tensor Design</title></titleStmt>
			<publicationStmt>
				<publisher></publisher>
				<date>12/01/2019</date>
			</publicationStmt>
			<sourceDesc>
				<bibl> 
					<idno type="par_id">10135559</idno>
					<idno type="doi">10.1038/s41598-019-55139-1</idno>
					<title level='j'>Scientific Reports</title>
<idno>2045-2322</idno>
<biblScope unit="volume">9</biblScope>
<biblScope unit="issue">1</biblScope>					

					<author>J. Irwin</author><author>S. Lindemann</author><author>W. Maeng</author><author>J. J. Wang</author><author>V. Vaithyanathan</author><author>J. M. Hu</author><author>L. Q. Chen</author><author>D. G. Schlom</author><author>C. B. Eom</author><author>M. S. Rzchowski</author>
				</bibl>
			</sourceDesc>
		</fileDesc>
		<profileDesc>
			<abstract><ab><![CDATA[]]></ab></abstract>
		</profileDesc>
	</teiHeader>
	<text><body xmlns="http://www.tei-c.org/ns/1.0" xmlns:xsi="http://www.w3.org/2001/XMLSchema-instance" xmlns:xlink="http://www.w3.org/1999/xlink">
<div xmlns="http://www.tei-c.org/ns/1.0"><p>Strain-coupled magnetoelectric (ME) phenomena in piezoelectric/ferromagnetic thin-film bilayers are a promising paradigm for sensors and information storage devices, where strain manipulates the magnetization of the ferromagnetic film. In-plane magnetization rotation with an electric field across the film thickness has been challenging due to the large reduction of in-plane piezoelectric strain by substrate clamping, and in two-terminal devices, the requirement of anisotropic in-plane strain. Here we show that these limitations can be overcome by designing the piezoelectric strain tensor using the boundary interaction between biased and unbiased piezoelectric. We fabricated 500 nm thick, (001) oriented [Pb(Mg 1/3 nb 2/3 )o 3 ] 0.7 -[PbTiO 3 ] 0.3 (pMn-pt) unclamped piezoelectric membranes with ferromagnetic Ni overlayers. Guided by analytical and numerical continuum elastic calculations, we designed and fabricated two-terminal devices exhibiting electric field-driven Ni magnetization rotation. We develop a method that can apply designed strain patterns to many other materials systems to control properties such as superconductivity, band topology, conductivity, and optical response.</p><p>Magnetoelectric materials systems possess a wide range of applications including non-volatile memories, magnetic field sensors, spintronics, tunable RF circuit elements, tunable optics, and biomedical devices <ref type="bibr">[1]</ref><ref type="bibr">[2]</ref><ref type="bibr">[3]</ref> . Significant effort has been devoted towards the few known materials exhibiting single-phase room temperature magnetoelectricity, but these materials have drawbacks such as weak magnetoelectric coupling or small electric polarizations <ref type="bibr">4</ref> . Composite magnetoelectrics, consisting of a ferromagnet coupled to a piezoelectric via strain, are a well-studied alternative to single phase magnetoelectrics. Composite magnetoelectrics have the largest reported magnetoelectric coupling constants and suitable electric polarizations, magnetic coercive fields, and saturation magnetizations. These characteristics make them highly promising inverse magnetoelectric effect device candidates, but up to this point such devices have been challenging to implement in thin-film form <ref type="bibr">2,</ref><ref type="bibr">[5]</ref><ref type="bibr">[6]</ref><ref type="bibr">[7]</ref> . In this work we design, fabricate, and characterize (001)-oriented, thin-film magnetoelectric membrane heterostructures based on the piezoelectric material [Pb(Mg 1/3 Nb 2/3 )O 3 ] 0.7 -[PbTiO 3 ] 0.3 (PMN-PT) <ref type="bibr">8,</ref><ref type="bibr">9</ref> . Giant piezoelectric coefficients and large electro-mechanical coupling have allowed PMN-PT based composite magnetoelectrics to achieve superior performance, for example in magnetic field sensors <ref type="bibr">3</ref> . By designing the piezoelectric tensor, we overcome previous limitations intrinsic to thin films, and demonstrate perpendicular electric field control of in-plane magnetization at low bias voltages.</p><p>The structure presented here overcomes two critical factors limiting thin-film composite magnetoelectrics. The first limitation arises from substrate clamping that greatly reduces the in-plane piezoelectric response of thin films <ref type="bibr">[10]</ref><ref type="bibr">[11]</ref><ref type="bibr">[12]</ref> , and the second limitation arises from the in-plane four-fold symmetry of most (001) pseudo-cubic piezoelectrics that precludes the anisotropic in-plane strain necessary for in-plane magnetization rotation. Substrate clamping has limited the majority of research on electric field control of magnetization in composite magnetoelectrics to bulk <ref type="bibr">2,</ref><ref type="bibr">7</ref> . Nanoscale patterning has been shown to partially address this by relaxing the island through its thickness <ref type="bibr">[13]</ref><ref type="bibr">[14]</ref><ref type="bibr">[15]</ref> . Membranes are free from substrate clamping <ref type="bibr">16,</ref><ref type="bibr">17</ref> and operate at low voltage while still providing for high device density. Special crystalline orientations <ref type="bibr">[18]</ref><ref type="bibr">[19]</ref><ref type="bibr">[20]</ref> , domain switching <ref type="bibr">[21]</ref><ref type="bibr">[22]</ref><ref type="bibr">[23]</ref> , and extra top electrodes <ref type="bibr">24</ref> have addressed the in-plane symmetry limitation, but our piezoelectric tensor design approach directly transforms biaxial piezoelectric strain into uniaxial strain that reorients in-plane magnetization, eliminating complexity and fabrication challenges. We demonstrate in-plane magnetization reorientation with out-of-plane electric fields, and develop design principles that can be used to generate specific strain patterns.</p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head>Results</head><p>experimental Approach. The membrane fabrication process starts from an epitaxial PMN-PT / SrRuO 3 bilayer on SrTiO 3 -buffered Si, and results in a piezoelectric membrane heterostructure on a soft polymer (Polydimethylsiloxane [PDMS]) coated glass slide (Fig. <ref type="figure">1</ref>, see Materials and Methods for details). Growth of high quality epitaxial PMN-PT/SrRuO 3 /SrTiO 3 heterostructures on 4&#176; miscut (001)-oriented Si substrates has been previously reported <ref type="bibr">25</ref> . A continuous Pt film sputtered onto the PMN-PT serves as the bottom electrode. The structure is attached Pt side down to soft PDMS coated glass, then the Si substrate is removed with a XeF 2 vapor phase etch, and the SiO 2 by ion-milling. This leaves behind sub-micron thick PMN-PT / SrRuO 3 . The exposed SrRuO 3 is patterned into top electrodes, defining the PMN-PT biased regions. A 35 nm thick Ni layer is deposited and patterned into regions in which we probe the magnetization rotation via Magneto-optic Kerr Effect (MOKE) measurements. A protective coating of SU-8 polymer and an overlayer of patterned Au allows probe tips to contact individual top electrodes. The cross section of the final heterostructure is shown in Fig. <ref type="figure">2a</ref>.</p><p>Structural, ferroelectric and piezoelectric characterization of the PMN-PT was performed on thin-film and membrane samples. High-resolution X-ray diffraction shows that the biaxiallly strained thin film PMN-PT relaxes towards bulk lattice constants after substrate removal (Supplementary Fig. <ref type="figure">S1</ref>). Release from the substrate also results in a slight increase in the PMN-PT (002) rocking curve from 0.4&#176; to 0.5&#176; due to the lattice constant relaxation (Supplementary Fig. <ref type="figure">S1</ref>). According to polarization-electric field hysteresis loops the PMN-PT has a remanent polarization of 20 &#956;C/cm 2 and a ferroelectric imprint of 50 kV/cm favoring the polarization pointing towards the SrRuO 3 (Supplementary Fig. <ref type="figure">S2</ref>).</p><p>A key aspect of our membranes is that the PMN-PT layer is continuous, with electrically biased regions (defined by patterned SrRuO 3 top electrodes) embedded in unbiased PMN-PT. A bias voltage applied between the continuous Pt bottom electrode and the patterned SrRuO 3 top electrode polarizes only this defined region of the PMN-PT, and we find that the intrinsic isotropic in-plane strain state is transformed by interaction with the surrounding unbiased PMN-PT into the anisotropic strain required to drive in-plane magnetic anisotropy. Anisotropic strain is present both inside and outside of the biased region, and the strain direction is spatially varying (Fig. <ref type="figure">2b</ref>). We refer to this interaction as boundary clamping and show that it can be used to design an electric field induced strain that controls the in-plane magnetization orientation in the Ni regions. Our measurements of membrane composite magnetoelectrics show electric-field induced uniaxial anisotropy and are in good agreement with our analytical and numerical analyses of the piezoelectric strain tensor in this constrained geometry. </p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head>experimental Results</head><p>Longitudinal magneto-optic Kerr effect (MOKE) magnetic hysteresis loops were used to measure strain-induced magnetic anisotropy in the Ni at different PMN-PT bias voltages. Applying the magnetic field along an easy magnetic direction will result in a square hysteresis loop as the magnetization jumps between orientations parallel and antiparallel to the applied field. Applied field along a hard direction rotates the magnetization away from the easy axis, resulting in a linear hysteresis loop with zero coercivity that saturates at an applied field H sat . The uniaxial magnetic anisotropy energy density K U can be estimated from the hard axis data with</p><p>where M s is the Ni saturation magnetization, and assuming coherent rotation <ref type="bibr">26</ref> .</p><p>Figure <ref type="figure">3a</ref> shows the bias dependence of MOKE hysteresis loops of a 300 &#956;m by 200 &#956;m Ni/SrRuO 3 rectangle that serves as top electrode for PMN-PT bias. In the top panel, the applied field magnetic field is along x1 , parallel to the long edge of a rectangle. As the applied bias is increased from 0 V to 8 V, the loops close from square to nearly linear, indicating the formation of a magnetic hard direction along x1 with an anisotropy energy of 1.2 kJ/ m 3 . In the bottom panel of Fig. <ref type="figure">3a</ref>, the measurement field is rotated by 90&#176; to be along x2 , parallel to the shorter edge of the pattern. As the applied bias increases, there is a small change in coercive field but no noticeable change in loop shape, showing that the x2 axis remains easy, independent of bias. These two measurements confirm that the piezoelectric strain has induced a new uniaxial anisotropy in the Ni layer along x2 . As Ni has a negative magnetostriction constant, x2 must be the most compressively strained direction in the biased region. At zero bias, the hysteresis loops for both field directions (and all others measured but not shown) are identical, indicating no intrinsic anisotropy in this sample. Strain-induced uniaxial magnetic anisotropy is expected to immediately induce a hard-axis response, with a magnetic anisotropy proportional to strain, rather than the incremental closing of the loops observed experimentally. We believe that our experimental results arise from strain-induced anisotropy competing against domain wall pinning, consistent with the relatively large 10 mT Ni coercive field, attributable to growth conditions. Devices on other samples showed an incremental increase in anisotropy energy with increasing bias voltage (Supplementary Fig. <ref type="figure">S6</ref>). Biased regions with aspect ratio A &#8800;1 generate excess strain along their shorter directions, which induces a magnetic easy direction (gold arrow). The strain distribution in both the biased (pink) and unbiased (green) regions can be considered in terms of local principal strains, shown with small axes indicating directions of principal strains &#949; 1 and &#949; 2 ). The gray squares represent undeformed infinitesimal patches and the black rectangles represent the same patches after deformation due to the piezoelectric response.</p><p>Figure <ref type="figure">3c,</ref><ref type="figure">d</ref> show spatial maps of the Ni coercivity measured with MOKE. A complete hysteresis loop was measured with the laser focused at each 10 &#956;m &#215; 10 &#956;m pixel and the magnetic field was aligned 30&#176; from the previously determined strain-induced hard axis direction. Shadowing of the laser by a wire bond prevented measurement with the magnetic field along x 1 or x 2 so an intermediate angle was chosen. At zero bias (Fig. <ref type="figure">3b</ref>), the coercive field is uniform and matches the zero-bias coercive field measured in Fig. <ref type="figure">2a</ref>. At a 6 V bias (Fig. <ref type="figure">3c</ref>), the coercive field drops considerably indicating loop closure and a strain-induced magnetic anisotropy. The loops don't close completely due to the 30&#176; misalignment with the hard axis. The coercivity is lower near the center of the pattern, and higher near the short edges, suggesting a larger anisotropy near the center of the electrode, as expected based on our analysis below.</p><p>In addition to the strains within the biased region of the PMN-PT, there is also significant strain outside of the biased region. The strain-induced magnetic anisotropies inside and outside of the biased region are qualitatively different. To probe this difference, we patterned a device with a grid of 60 &#956;m by 80 &#956;m Ni islands, each free to respond independently to local strains, placed on and around a 300 &#956;m by 200 &#956;m SrRuO 3 electrode. MOKE magnetic hysteresis loops are shown for two nearby Ni islands at 0 V and 5 V, one inside (Fig. <ref type="figure">4a</ref>) and one outside (Fig. <ref type="figure">4b</ref>) of the biased region. Both islands have square hysteresis loops at zero bias with the applied field along x2 . Due to different growth conditions, the Ni in the two islands in Fig. <ref type="figure">4a</ref> and b have as-grown magnetic anisotropy along x2 , in contrast to the Ni in the sample measured in Fig. <ref type="figure">3</ref> which was magnetically isotropic. At 5 V, the Ni island inside the biased region has an unchanged hysteresis loop, matching the behavior of the larger Ni rectangle shown in Fig. <ref type="figure">1a</ref> (bottom panel). The Ni island outside the bias region, under a 5 V bias, develops an 0.84 kJ/m 3 anisotropy parallel to the long edge and perpendicular to the anisotropy induced inside the biased region. This 90&#176; difference in anisotropy is consistent with our detailed analysis presented below, but can also be understood qualitatively: when the biased PMN-PT compresses inwards, it stretches the unbiased region. The magnetization in the compressed region aligns parallel to the axis of compression (Fig. <ref type="figure">4a</ref>, easy axis along x 2 &#710;), and in the stretched region aligns perpendicular to the axis of tension (Fig. <ref type="figure">4b</ref>, easy axis along x1 ). </p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head>Discussion</head><p>Our magnetoelectric measurements demonstrate that piezoelectric strain is responsible for inducing, via magnetoelasticity <ref type="bibr">27</ref> , a magnetic easy axis along the shorter direction of rectangular electrodes. This would not occur without the boundary clamping of the biased PMN-PT by the surrounding unbiased PMN-PT. Here we develop an analysis that relates the piezoelectric strain, boundary clamping, and magnetic anisotropy, and which allows for the design of an electric field-dependent magnetic anisotropy pattern in the Ni layer through piezoelectric tensor design.</p><p>A bias applied across the thickness of the PMN-PT generates strain in the PMN-PT through the converse piezoelectric effect. Normal (non-shear) strains in cubic piezoelectrics are characterized by two piezoelectric tensor components, d 33 &gt; 0 and d 31 &lt; 0, which in this geometry respectively describe the elongation parallel and perpendicular to the applied electric field. Because of its tetragonal symmetry when polarized along x3 , an unconstrained sheet of PMN-PT responds equally along x1 and x2 (i.e. d 31 = d 32 ), creating isotropic strain. However, when only a small region of the membrane is biased, its contraction is constrained by the surrounding unbiased PMN-PT, resulting in anisotropic response. We find that the effect of this boundary clamping can be described with effective (subscript eff) piezoelectric tensor components of the biased region, with d 32,eff &#8800; d 31,eff . This modification leads to strain-dependent uniaxial magnetic anisotropy.</p><p>This magnetic anisotropy induced by the applied bias depends on the in-plane components of the strain tensor, which are spatially varying due to the boundary clamping. Locally, every two-dimensional strain distribution has a direction of maximum strain and minimum strain, referred to as the first and second principal strain directions. The notation &#949; 1 and &#949; 2 is used here to denote the magnitude of the first and second principal strains. In terms of the principal strains, the induced anisotropy energy in the presence of an arbitrary strain distribution is</p><p>where &#955; S and Y Ni are the saturation magnetostriction constant (-32.9 ppm) and Young's modulus (220 GPa) of polycrystalline Ni <ref type="bibr">27</ref> . This means that however complex the strain distribution, it locally induces a uniaxial anisotropy, with direction and magnitude determined by the principal strains of the strain tensor. Here the anisotropy axis is parallel to the second principal strain direction, because this is the most compressed direction and Ni has a negative &#955; S . Figure <ref type="figure">2b</ref> schematically shows the principal strains at three infinitesimal regions in the biased and unbiased regions of a piezoelectric membrane. Upon applying a bias, the gray (undeformed) square patches are stretched or compressed into the black rectangular patches, each with its own principal strain directions. We can estimate the strain difference &#949; 1 -&#949; 2 at the center of the biased region from Eq. ( <ref type="formula">1</ref>) using the values of K U from our MOKE hysteresis loops. Considering only strain-induced anisotropies, the hard axis measurement in Fig. <ref type="figure">3a</ref> gives &#949; 1 -&#949; 2 = 11 ppm at 8 V bias, and that of Fig. <ref type="figure">4b</ref> gives &#949; 1 -&#949; 2 = 78 ppm at 5 V bias. The effective piezoelectric constants may also be estimated as the strain difference per applied electric field, giving d 31,effd 32,eff = 6.9 pm/V.</p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head>Analysis.</head><p>We find that strain patterns in our piezoelectric membranes can be understood by building on a continuum elasticity theory first developed by Eshelby <ref type="bibr">28</ref> to describe the elastic behavior of precipitates in materials. An exactly ellipsoidal region embedded in an elastic media will strain anisotropically in response to an isotropic internal stress, with the strain exactly uniform inside the ellipsoid. The strain is largest along the shortest axis of the ellipsoid. This is in agreement with our experimental results: the biased regions in our samples undergo uniform stress from their piezoelectric response, and our MOKE measurements indicate that the largest compressive strain lies along the shorter axis of rectangular patterns, in agreement with Eshelby's model.</p><p>Inside an infinite elliptical cylinder with axes a and b, respectively along x1 and x2 , the strain response to an electric field along the cylinder axis is 29 . The resulting first and second principal strains are &#949; 11 (along x1 ) and &#949; 22 (along x2 ). The magnetic anisotropy induced by this strain distribution, as a function of aspect ratio and applied electric field, is found from Eqs. ( <ref type="formula">1</ref>) and ( <ref type="formula">2</ref>) to be 3  31   11   Using bulk materials constants <ref type="bibr">30</ref> in this model yields K U = 1.1 kJ/m 3 for an 8 V bias across a 3:2 aspect ratio ellipse, close to the measured value 1.2 kJ/m 3 for our rectangular electrodes. This order of magnitude agreement suggests that far inside the pattern edges the aspect ratio primarily determines the effect of boundary clamping on the electric field induced magnetic anisotropy. According to this analysis, the magnitude of the magnetic anisotropy is independent of the absolute size of the biased region, suggesting that lateral electrode dimensions much smaller than the 100 &#956;m scale used here would still be effective. However, the assumptions of a sharply defined boundary region and a purely out-of-plane electric field break down for lateral electrode sizes smaller than the piezoelectric thickness due to electric field fringing. This would likely modify the effects described here.</p><p>Finite element continuum elastic simulations were performed to address the rectangular biased regions used in our experiments, mapping strains and the resulting magnetic anisotropy (Fig. <ref type="figure">4c</ref>). All layers of the structure shown in Fig. <ref type="figure">2a</ref> except the Au and SU-8 were included in the simulation, using bulk values for the elastic, piezoelectric and dielectric tensors of PMN-PT <ref type="bibr">30</ref> . Figure <ref type="figure">4c</ref> shows the strain-induced magnetic anisotropy energy per applied voltage (color) and anisotropy direction (white lines) on the surface of the PMN-PT layer. The computed anisotropy predominantly perpendicular to the long edge reproduces the experimental results of Fig. <ref type="figure">4a,</ref><ref type="figure">b</ref>. The change in direction near the short edge coincides with very small anisotropy magnitude, and so is difficult to detect experimentally. The computed 0.45 kJ m -3 V -1 magnitude in the large central portion of the biased region predicts a 3.6 kJ m -3 anisotropy energy density at 8 V, three times the experimental value. The computed anisotropy is largest near the center, consistent with the experimental spatial maps of Fig. <ref type="figure">3c</ref>.</p><p>We also simulated a series of elliptical electrodes with varying aspect ratios to compare with the Eshelby approach. Figure <ref type="figure">3d</ref> shows that the simulated and analytical anisotropy energies have the same</p><p>dependence on aspect ratio. However, the analytic result of Eq. ( <ref type="formula">3</ref>) describe an infinite cylinder of PMN-PT, and the simulation the experimental two-dimensional composite sheet. The two y-axis scales in Fig. <ref type="figure">4d</ref> indicate that this difference results in different predicted anisotropy energy magnitudes, but the dependence on aspect ratio is captured by the analytic result.</p><p>According to finite element calculations, the area of largest uniaxial strain is just outside of the biased region boundary (Fig. <ref type="figure">4c</ref>). Analytical solutions <ref type="bibr">31</ref> for the strain outside of elliptical precipitate inclusions confirm that the largest uniaxial strains are concentrated on the most curved portion of the boundary. The measured anisotropy direction of the Ni island outside the biased region (Fig. <ref type="figure">4b</ref>) matches the calculated anisotropy parallel to the long edge (Fig. <ref type="figure">4c</ref> boxed in black) and the direct phase-field calculation of the magnetization direction (Supplementary Fig. <ref type="figure">S5</ref>) for that location. We did not experimentally find a significant difference in the induced anisotropy energy inside and outside of the biased region, likely due to pre-existing magnetic anisotropy and domain pinning in the Ni that makes H sat a coarse method for measuring anisotropy energy. A sharp strain drop off outside the biased region would be desirable in a dense array of electrodes to avoid mechanical "cross-talk". We estimate that the required separation between devices would be on the order of the electrode's largest dimension, and less separation is required for higher aspect ratio devices. Far away from the boundary, the exterior strains drop off as 1/|x| 2 (see Supplementary equations S8 to S15).</p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head>conclusions</head><p>The preceding analysis, and that summarized in the Supplementary Information, leads to a set of guidelines for setting magnetoelectric response in piezoelectric membrane composites using piezoelectric tensor design. An elongated single electrode generates, in its interior, uniaxial compressive strain and magnetic anisotropy that increases with aspect ratio, and is predominantly oriented along the short axis. Ellipsoidal biased regions have exactly uniform interior strains (Supplementary Fig. <ref type="figure">S3</ref>), with about sixty percent of the limiting anisotropy value obtained at an aspect ratio of 4:1. Substantial further increases require large increases in aspect ratio. Rectangular regions generate about 20% more uniaxial strain than ellipses of the same aspect ratio (Supplementary Fig. <ref type="figure">S4</ref>), but the strain is less uniform in rectangles. The maximum uniaxial tensile strain is located outside highly curved boundaries and is at least twice as large as the interior uniaxial strain, but at the cost of reduced spatial uniformity (Supplementary equations S8 to S15). In the case of a straight boundary, the exterior magnetic anisotropy is perpendicular to the interior anisotropy. These rules allow for the design of particular anisotropy magnitudes and directions using boundary shape and layout.</p><p>Piezoelectric membrane composites are positioned to take advantage of interest in freestanding films and the number of available fabrication techniques <ref type="bibr">16,</ref><ref type="bibr">17,</ref><ref type="bibr">32,</ref><ref type="bibr">33</ref> . Our results here demonstrate the fundamental principles of piezoelectric tensor design for magnetoelectric coupling in membrane composites, and optimization of the biased region geometry will likely realize even higher ME coupling. As any Si compatible piezoelectric and any ferromagnet that can be deposited at room temperature may be used with our fabrication process, the optimum magnetoelectric response would be obtained with a large piezoelectric response membrane and high magnetostriction magnetic layer <ref type="bibr">34</ref> . Several theoretical proposals for inducing 180&#176; in-plane magnetization rotation in bulk composite magnetoelectrics using spatially varying electric fields have been put forth <ref type="bibr">[35]</ref><ref type="bibr">[36]</ref><ref type="bibr">[37]</ref> . Piezoelectric membranes offer an alternative, thin-film platform for realizing such proposals using the design guidelines developed here. We also expect that these structures can be used as sensors, with a piezoelectric readout. Although we have focused on in-plane magnetization manipulation, the biaxial strain present in square or circular devices may also be able to control the out-of-plane magnetization of a ferromagnetic overlayer with perpendicular magnetic anisotropy <ref type="bibr">38,</ref><ref type="bibr">39</ref> . Additionally, integration of other materials with piezoelectric membranes would allow for electric field control of, for instance, superconducting T C 40-42   , band topology <ref type="bibr">[43]</ref><ref type="bibr">[44]</ref><ref type="bibr">[45]</ref> , conductivity <ref type="bibr">46</ref> , and optical properties <ref type="bibr">47</ref> with designed strain patterns.</p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head>Materials and Methods</head><p>Membrane fabrication. Figure <ref type="figure">1</ref> is the schematic of the fabrication procedure for the PMN-PT membrane devices. Here we will describe the method in detail. Growth of high quality PMN-PT (001) thin films started with a (001) Si wafer with a 4&#176; miscut towards (110) and a 20 nm buffer layer of STO. First, 100 nm of SRO was grown using 90&#176; off-axis rf-magnetron sputtering <ref type="bibr">48</ref> at 100 W power and 600 &#176;C. A mixture of Ar and O 2 gas, flown at 12 sccm and 8 sccm respectively, supplied a working pressure of 200mTorr. PMN-PT films were then grown using a misaligned parallel dual planar magnetron sputtering technique <ref type="bibr">49</ref> with substrate rotation with 100 W power at 625 &#176;C. A mixture of Ar and O 2 gas, flown at 17 sccm and 3 sccm respectively, supplied a working pressure of 500 mTorr for PMN-PT growth. A 100 nm layer of Pt was then deposited on top of PMN-PT by DC magnetron sputtering. The heterostructure was annealed in O 2 at 300 &#176;C for 30 minutes to reduce residual stress in the Pt film. The Si substrate was then mechanically polished to reduce the thickness from 300 &#956;m down to 100 &#956;m to reduce total etching time during the later XeF 2 dry etching. After polishing, Polydimethylsiloxane (PDMS), with a 10:1 mixture ratio of monomer to crosslinking agent, was spin-coated onto a glass slide at 5000 rpm for 10 s, resulting in a thickness of approximately 30 um. The thin film heterostructure was then placed Pt-side down onto the uncured PDMS, leaving the Si substrate exposed, and the sample was placed under vacuum for a minimum of 5 hours to remove air bubbles from between the Pt and PDMS layers. After the vacuum treatment, the PDMS was then cured on a hot plate for 1 hour at 100 &#176;C.</p><p>Once the PDMS was cured, the sample was ready for Si removal. Prior to XeF 2 etching of Si, a 15 second plasma etch using CF 4 and O 2 , flowing at 45 sccm and 5 sccm, respectively, to a pressure of 40mTorr, was performed to remove any moisture on the sample, as well as any native SiO 2 present on the Si substrate. The Si substrate was then completely removed via XeF 2 etching. The XeF 2 etching system was performed in a SPTS Xetch e1 XeF 2 etcher system. The system exposes the samples to XeF 2 in a cyclic mode, and the recipe used here was chosen to maximize the etch rate for complete removal of the Si substrate. The recipe exposed the samples to 4 Torr of XeF 2 for two-minute periods, followed by pumping down to 0.8 Torr between cycles for a continuous etch before the next cycle began. Due to the exothermic nature of the reaction of XeF 2 with Si, the pressure in the chamber rises during the two-minute etch cycles. When the Si is completely removed, the pressure increase is notably absent during an etch cycle, signaling that the etching is complete.</p><p>After Si removal, the STO buffer layer was removed via Ar + ion-milling. The SRO layer was then patterned into various geometries using photolithography and wet etching with a 0.4 M NaIO 4 solution. A 35 nm layer of Ni was deposited by DC Magnetron sputtering, and photolithography was performed to pattern the Ni with a Transene Ni Etchant Type 1 wet etchant. A SU-8 protection layer was applied by spin-coating at 5000 rpm for 40 s, resulting in a thickness of 2um, followed by photolithography patterning. Finally, 30 nm of Au was deposited via DC Magnetron sputtering and patterned via photolithography, and Transene TFA Au wet etchant was used to make the "lifted" Au electrodes.</p><p>finite-element Simulations. Finite element calculations were performed with COMSOL Multiphysics TM . Simulations were performed using the layers and thicknesses from Fig. <ref type="figure">2a</ref>. The sheet of PMN-PT and back electrode were 1.4 &#956;m diameter to simulate a small biased region surrounded by a large unpolarized membrane. No mechanical constraints were applied to any surfaces, simulating an unconstrained membrane. The stiffness tensor and piezoelectric coefficients used for PMN-PT may be found in Table <ref type="table">2</ref> of reference <ref type="bibr">30</ref> . The stress-charge form of the piezoelectric constitutive relations was used:</p><p>where D i , E i , &#963; ij , &#949; kl , &#961; f , e ijk , c ijkl , &#954; ij are the electric displacement, electric field, stress tensor, strain tensor, free charge density, piezoelectric coupling tensor, stiffness tensor and relative permittivity, respectively. A control simulation was performed with 700 nm of Si added below the Pt back electrode, and with a zero-strain constraint on the bottom face (furthest from the PMN-PT) of Si to simulate substrate clamping. In this simulation, the volume-averaged &#949; 11 -&#949; 22 in the Ni film dropped to 0.2 ppm from the unconstrained value of 34 ppm, using a 300 &#956;m by 200 &#956;m rectangular biased region and a 20 kV/cm electric field.</p><p>Longitudinal MoKe Measurements. The sample was mounted between the poles of an electromagnet and a red HeNe (632 nm) laser was reflected off of the sample surface at approximately 45&#176; from normal incidence. The beam was focused to an approximately 10 &#956;m spot using an achromat. The reflected beam's polarization was rotated to 45&#176; from p-polarized with a half-wave plate and then the s-and p-polarized components were measured with a differential balanced photodetector. The differential signal is proportional to the Kerr polarization rotation. Spatial mapping was achieved by mounting the sample on a two-axis linear piezoelectric motion stage and scanning the sample under the focused beam.</p></div><note xmlns="http://www.tei-c.org/ns/1.0" place="foot" xml:id="foot_0"><p>Scientific RepoRtS | (2019) 9:19158 | https://doi.org/10.1038/s41598-019-55139-1</p></note>