<?xml-model href='http://www.tei-c.org/release/xml/tei/custom/schema/relaxng/tei_all.rng' schematypens='http://relaxng.org/ns/structure/1.0'?><TEI xmlns="http://www.tei-c.org/ns/1.0">
	<teiHeader>
		<fileDesc>
			<titleStmt><title level='a'>The influence of processing parameters on piezoelectric and dielectric properties of dome-shaped composite PZT-epoxy actuators</title></titleStmt>
			<publicationStmt>
				<publisher></publisher>
				<date>2020 September</date>
			</publicationStmt>
			<sourceDesc>
				<bibl> 
					<idno type="par_id">10301008</idno>
					<idno type="doi">10.1016/j.jmapro.2020.05.036</idno>
					<title level='j'>Journal of manufacturing processes</title>
<idno>1526-6125</idno>
<biblScope unit="volume">57</biblScope>
<biblScope unit="issue"></biblScope>					

					<author>W. Hoyt Du</author>
				</bibl>
			</sourceDesc>
		</fileDesc>
		<profileDesc>
			<abstract><ab><![CDATA[Thick film dome-shaped composite PZT-epoxy structures have been fabricated using a modified sol gel and spin coating technique. Processing parameters and polarization technique (Corona versus contact polarization) have been studied to elucidate their influence on piezoelectric and dielectric properties. The volume fraction of PZT was varied from 0.0 to 0.7 and the highest values for the longitudinal piezoelectric coefficient, effective dielectric constant (@1kHz) and dielectric loss (@1kHz), were 11.1 pC/N, 28.7 and 0.004 respectively for the PZT volume fraction equal to 0.7. The piezoelectric strain coefficient for this dome structure was 7 times higher than previously reported values for a composite PZT-epoxy dome structure of similar structure and composition. The sample morphology was examined with the aid of scanning electron microscopy (SEM) images. The piezoelectric strain coefficients, capacitance, and effective dielectric constant increased with increasing PZT volume fraction, in addition to the surface roughness. Samples that were Corona poled facilitated higher polarization voltages (45 kV/mm and 70 kV/mm) and resulted in higher values of piezoelectric strain coefficients. Investigation of composite structures such as these will advance the development of curved and hemispherical piezoelectric actuators with enhanced displacement and mechanical properties.]]></ab></abstract>
		</profileDesc>
	</teiHeader>
	<text><body xmlns="http://www.tei-c.org/ns/1.0" xmlns:xsi="http://www.w3.org/2001/XMLSchema-instance" xmlns:xlink="http://www.w3.org/1999/xlink">
<div xmlns="http://www.tei-c.org/ns/1.0"><head>Introduction</head><p>Piezoelectric ceramics are widely employed as sensors and actuators because of their ideal electromechanical properties. Ceramic piezoelectric actuators are typically simple in structure and highly reliable <ref type="bibr">[1]</ref>; render large actuation forces and rapid response times, and consume minimal power during operation <ref type="bibr">[2]</ref>. Despite these advantages, piezoelectric ceramics are brittle in nature, which limits their operational strains <ref type="bibr">[3]</ref>, operational loading frequency, cycle life and compatibility to applications requiring complex shapes. These poor mechanical properties limit their effective application to devices such as; hydrophones <ref type="bibr">[4,</ref><ref type="bibr">5]</ref>, static and vibration based energy harvesting devices <ref type="bibr">[6,</ref><ref type="bibr">7]</ref>, surgical tactile sensors <ref type="bibr">[2,</ref><ref type="bibr">8,</ref><ref type="bibr">9]</ref>, biomedical scaffolds <ref type="bibr">[10,</ref><ref type="bibr">11]</ref> and synthetic jet actuators <ref type="bibr">[12]</ref>. Piezoelectric polymers, such as polyvinylidene fluoride (PVDF) are flexible, lightweight and have low acoustic and mechanical impedance, but suffer from low piezoelectric properties (d 31 &#8764;6-28 pC/N <ref type="bibr">[13,</ref><ref type="bibr">14]</ref>). Composite piezoelectric materials leverage the ideal characteristics of disparate materials with dissimilar characteristics to tune the piezoelectric and dielectric properties towards increasing the design degrees of freedom for the application to advanced devices and systems.</p><p>Interest in dome and curved shaped piezoelectric devices has increased because these structures demonstrate higher deformation <ref type="bibr">[15]</ref> and electromechanical conversion accuracy <ref type="bibr">[16]</ref> in comparison to planar actuators <ref type="bibr">[17]</ref><ref type="bibr">[18]</ref><ref type="bibr">[19]</ref><ref type="bibr">[20]</ref>. A summary of work performed in domeshaped piezoelectric devices is presented in Table <ref type="table">1</ref>. Dome-shaped piezoelectric actuators can also achieve large loading <ref type="bibr">[21]</ref> and large electro-induced displacements <ref type="bibr">[16]</ref> in comparison to planar bimorph and multilayer actuators. In this work, dome-shaped 0-3 connectivity piezoelectric composites comprised of lead zirconate-titanate (PZT) and epoxy were fabricated using a combination sol gel mix, spin coat, and cast method. The volume fraction of the PZT was varied from 0.1 to 0.7. The influences of the viscosity (composite mixture before the spin coat process) and polarization voltage, on the effective composite piezoelectric and dielectric properties were investigated.</p><p>Less than a handful of groups have successfully fabricated dome shaped actuators using a combination sol gel engineered approach., which allows for tremendous flexibility in the processing of these types of structures. In our previous work <ref type="bibr">[22]</ref>, a sol-gel and spin-coating technique was used to fabricate 0-3 composite PZT-Epoxy dome-shape structures with filler volume fractions ranging from 10% to 70%. The values for piezoelectric strain coefficients, d 33 and d 31 , capacitance, C, and effective dielectric constant, &#949;, were 1.06 pC/N, 0.74 pC/N, 6.0 pF and 76.1 respectively at 70% volume fraction of PZT. It was determined that these devices had the potential to be applied as sensor/actuators, capacitors and low-power energy harvesting devices <ref type="bibr">[22]</ref>. While the effective dielectric constant was comparable to the range of other works (32 to 71 <ref type="bibr">[23,</ref><ref type="bibr">24]</ref>), the d 33 values were low compared to other's (4pC/N to 24.8 pC/N <ref type="bibr">[23]</ref><ref type="bibr">[24]</ref><ref type="bibr">[25]</ref>). The lower piezoelectric strain coefficient values were attributed to PZT agglomerations and air pockets within the matrix, which hindered the effectiveness of the polarization process. The purpose of this work is to investigate how processing techniques (polarization and spin coat deposition profile) influence the piezoelectric and dielectric materials properties.</p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head>Materials and methods</head><p>The results from optimized (final after all studies were completed) processing procedure are presented and compared to the results from our prior work <ref type="bibr">[22]</ref>. In order to achieve the optimized processing steps described in this paper, a parametric study was performed to identify the influence of several processing parameters on the resulting piezoelectric and dielectric properties of the dome-shaped devices. The modified procedure for the fabrication of the piezoelectric dome structures is derived herein and is based on a Spin -Speed/Time Profile study and Deposition Technique Study. The dielectric constant, dissipation factor, resistivity, normalized impedance and phase of epoxy single-phase sample are measured over the frequency range of 2 kHz to 20 MHz. The longitudinal and transverse piezoelectric coefficients d 33 and d 31 were measured along with the capacitance to examine the relationship between PZT volume fraction and device performance.</p><p>This section is divided into four parts: Section 2.1: Materials, Section 2.2: Experimental Methodology, Section 2.3: Piezoelectric and Dielectric Characterization. In Session 2.1 an overview of the materials used for sample preparation is provided. In Section 2.2, overviews of the original and modified fabrication methods are presented, and in Section 2.3, the piezoelectric and dielectric characterization process is described.</p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head>Materials</head><p>The materials used in the previous work <ref type="bibr">[31]</ref> and this work were maintained. In Table <ref type="table">2</ref>, the physical, dielectric and piezoelectric properties of the lead zirconate titanate (Pb(Zr Ti )O</p><p>x (1-x) 3 -855, Navy VI) and the two-part epoxy -DGEBA, EpofixTM Cold-setting embedding resin (purchased from APC International and Electron Microscopy Sciences, respectively) are detailed. An overview of the fabrication process from the previous work <ref type="bibr">[31]</ref> is presented in Fig. <ref type="figure">1</ref>. The values for the PZT are for bulk PZT as published by APC International. The values for the DEGBA were determined from an epoxy dome structure that was</p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head>Table 1</head><p>Overview of the state of the art in fabrication techniques and piezoelectric and displacement performance of dome-shaped piezoelectric devices. Actuator -Unimorph(70% PZT)/spin-coating <ref type="bibr">[22]</ref> 76.1 @110 Hz  fabricated using the same steps as defined herein with 0% PZT. In this paper, several modifications to the previous fabrication process were performed: 1) the addition of a desiccation step to eliminate air bubbles; 2) a modified spin coat deposition process based on observations from the study described in Section 2.2.1: Spin Coat Deposition Speed Study and Time Profile Study and Section 2.2.2: Sol Gel Layering Study; 3) maintenance of the sol gel viscosity to be within a range of 150-200 mPa s; and 4) the implementation of a Corona polarization process instead of the Contact Parallel Plate polarization process. The new fabrication procedure used for this paper is depicted in Fig. <ref type="figure">2</ref>.</p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head>Methods</head><p>An overview of the fabrication methodology that was used for this work is provided in Fig. <ref type="figure">2</ref>. The volume fraction of PZT was varied from 0.0 to 0.7. First, the PZT powder was ball milled for 24 h, where the mean diameter of the PZT after the ball mill step was observed to be &#8764;0.97 microns. Next, adequate amounts of the PZT and the epoxy were weighed and mixed with ethanol (15 ml) by hand. The mixture was sonicated for 2 h, desiccated for 4 h, and then sonicated for an additional hour. Samples that had initial viscosity values less than 150mPas were subjected to additional sonication until the final viscosity was within the range of 150 to 200 mPas @100rpm. The resulting mixture was spin coated onto a dome shaped metal substrate. The substrate was stainless steel, Type 304, (Alfa Aesar, Ward Hill, MA, USA). The dome shaped stainless steel substrate was made by pressing the stainless-steel substrate in a mold at a pressure of 500 psi for 15 min at room temperature.</p><p>The dimensions for the dome structure are provided in Fig. <ref type="figure">3</ref>. Once deposited, the dome shaped films were cured on a hot plate at 75 &#176;C for 8 h.</p><p>The piezoelectric dome structures were heated using a hot plate for 10 min at 75 &#176;C prior to corona polarization. Samples that comprising 10%-70% volume fraction of PZT were polarized at 45 kV/mm at a temperature of 75 &#176;C in air for 30 min. The temperature of 75 &#176;C was selected to obtain optimal cure quality and polarization characteristics. In particular, the curing agent used for the diglycidyl ether bisphenol A (DEGBA) liquid formulation achieves rapid reactivity above 70 &#176;C, where it has been found with the aid of Differential Scanning Fig. <ref type="figure">1</ref>. Overview of the original method used from our previous work <ref type="bibr">[22]</ref>. Fig. <ref type="figure">2</ref>. Overview of the method of fabrication used for this work. Appropriate amounts of PZT, DEGBA and ethanol were weighed and then mixed and sonicated for 2 h. The mixture was subsequently dessicated for 4 h and sonicated for an additional hour. The binder was then added to the mixture and sonicated again. The final mixture was spined coated onto the dome-shaped stainless steel substrate and cured at 75 &#176;C. Samples were corona polarized. Calorimetry (DSC) analysis <ref type="bibr">[33,</ref><ref type="bibr">34]</ref> that beyond this temperature there is an exothermic peak observed prior to an endothermic trough, which indicates the rapid crystallization of the DEGBA. The crystallization process of DEGBA is both quick and energetic, which allows for a quick return to a solid steady-state condition. However, the inclusion of a fillers increases the energy barrier during the cure process. This insight was coupled with the fact that the effectiveness of the polarization technique is dependent upon domain wall motion, which can be pinned by grain boundaries which develop electric fields due to crystallographic mismatches <ref type="bibr">[35]</ref> that are enhanced at escalated reaction rates and subsequent solidification of the epoxy at elevated temperatures. Another set of samples (0.10, 0.20 and 0.30 vol fractions of PZT) were poled at 70 kV/mm at 75 &#176;C for 30 min. The latter set of samples could be poled at a higher poling voltage due to the smaller volume fractions of PZT, while the former samples could not be polarized at the higher voltage. No top electrodes were used during the corona polarization process. The samples were wrapped in aluminum foil (to remove residual charges) and set aside for 24 h after the polarization process.</p><p>The film thickness of the samples was measured using mechanical calipers at 5 locations on the dome structure. These recorded thickness values were averaged, and these thicknesses were validated with the aid of SEM micrographs of the cross section of selected samples.</p><p>Two dependent studies were performed to determine the optimized deposition speed and time profile and deposition viscosity and layering for the dome-shaped structures. The two studies, speed/time and deposition layer were decoupled to independently understand the processing influence of sample performance. These two studies are described in Sections 2.2.1 and 2.2.2.</p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head>Spin coat deposition speed and time profile study</head><p>The spin coat speed and time increment studies were performed to ascertain the ideal characteristics for the spin coat speed and deposition step time for the fabrication procedure described in Fig. <ref type="figure">2</ref>. An overview of the spin coat speed/time interval profiles studied are provided in Fig. <ref type="figure">4</ref>. This study was done on samples with 0.50 vol fraction of PZT, where the viscosity of the sol gel was maintained at &#8764;164.5 mPas @ 100 rpm. The amount of sol gel and total spin coat time was maintained at 2 mL and 220 s, respectively.</p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head>Sol gel deposition layer study</head><p>A Deposition Layer Study was performed because at PZT volume fractions less than and equal to 0.40, no piezoelectric strain coefficients were detected for samples that were subjected to the polarization process at 45 kV/mm and with sol viscosities between 150-200 mPa s. Hence, this study was conducted on samples where the volume fraction of PZT was a minimum of 0.40. The influences of the number of deposition layers, time interval between layer deposition and sol gel viscosity were examined.</p><p>An overview of the Deposition Layer Study is provided in Fig. <ref type="figure">5</ref>. The steps before deposition were kept the same as those described in Fig. <ref type="figure">2</ref>. For each sample fabricated, the amount of sol gel was maintained at 2 ml. The samples were fabricated at viscosities that were equal to 150, 248.7 and 299 mPas (the spin coat and deposition equipment was operated at 100 rpm). The films were deposited in one, two or three layers as shown in Fig. <ref type="figure">5</ref>. The total amount of sol gel was maintained for each process and the same speed/interval profile was maintained for each layer deposition step. The datum sample included one deposition layer, where the measured viscosity prior to the application of the single layer was 150mPas.</p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head>Material characterization</head><p>In this work, the mechanisms that influence the piezoelectric and dielectric properties of composites are investigated as a function of the volume fraction of PZT with the aim of understanding the influence of fabrication technique on the aforementioned properties. The films were characterized in terms of their dielectric spectra, piezoelectric strain coefficients, dielectric loss (tan &#948;), impedance spectra and viscosity. The dynamic viscosity of the mixture was then measured using a Brookfield DV-E viscosity meter. The piezoelectric strain coefficients, d 33 and d 31 were measured at the frequency of 110 Hz using the PiezoMeter PM300. Frequency dependent capacitance, dielectric loss, resistance, conductance, impedance and phase spectra were measured with an impedance analyzer, HP 4194A Impedance Analyzer. The measured values were used to calculate the dielectric constant, resistivity and normalized impedance. The impedance was normalized with the area and thickness. The piezoelectric strain coefficients and the capacitance were initially measured without a top electrode. Then, electrically conductive silver paste was added to some samples for the top electrode, and the d 33 values were recorded again and compared to the values where no top electrode was used. The dielectric impedance, phase angle, capacitance and dielectric loss (tan &#948;) were measured as a function of frequency (2 kHz to 20 MHz) on samples that used aluminum tape as the top electrode. Ultimately, the aluminum tape was used instead of silver paste because the paste caused some samples to short circuit. The aluminum tape electrode was triangular in shape with an average area equal to 18.5 mm 2 . The dielectric constant was calculated using Eq. 1. In Eq. 1, &#949; r is the relative dielectric constant, &#949; 0 is dielectric constant of a vacuum</p><p>The dielectric constants that were calculated from the measured values and were compared to an analytical model proposed by Furukawa <ref type="bibr">[36]</ref>, expressed in Eq. 2. In Eq. 2, &#949;, &#949; &#949; , 1 2 and &#8709;, are the effective dielectric constant of the composite, the dielectric constant of the epoxy matrix, the dielectric constant of the PZT, and the volume fraction of the inclusions, respectively.</p><p>The piezoelectric strain coefficient was compared to the coefficients predicted by Furukawa's <ref type="bibr">[37]</ref> analytical expressed in Eq. 3. In Eq. 3, d 33 is the piezoelectric strain coefficient,</p><p>In Eq. 3, c c , 1 and c 2 are the Young's Moduli of the composite, matrix and   second layers (for Process B) was three minutes. Similarly, three sets of samples were prepared using Processes C and D, and the viscosities were measured to be equal to 150, 248.7 and 299 mPas, respectively. The time intervals between the deposition of the first and second layers were 9 and 3 min for Process C, and 18 and 5 min for Process D, respectively. Three layers of deposition were used for Processes E and F, and three sets of samples were prepared at viscosity values equal to 150, 248.7 and 299 mPas, respectively. The time increments between the deposition of the layers for Process E were equal to 29, 3 and 3 min, and equal to 44, 5 and 5 min, respectively for Process F. Process G was implemented for the fabrication of two data sets of samples at viscosities equal to 248.7 and 299 mPas, respectively. A single time interval of 63 min was taken prior to the deposition of the first and only layer.</p><p>The piezoelectric dome shaped composites underwent polarization following the process described in Fig. <ref type="figure">2</ref> after the layer(s) were deposited onto the stainless-steel substrates and pressed. The devices were Corona polarized at 45 kV/mm and were allowed to age one day before the measurement of the piezoelectric strain coefficients, thicknesses and dielectric properties.</p><p>The fractured surface morphology and Electron Dispersion Spectroscopy (EDS) of the samples were studied with using micrograph images obtained from a Scanning Electron Microscope (SEM) (FESEM ZEISS 982) to ascertain the distribution of the PZT filler in the matrix, PZT filler mean size, degree of separation of particles, particle morphology, composite porosity and agglomeration.3.</p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head>Results and Discussion</head><p>The results obtained in this work were compared to our previous work and analytical models at corresponding volume fractions. The piezoelectric coefficients with silver paste electrodes were compared to those without top electrodes, our previous work and an analytical model. Piezoelectric coefficients d33 and d31 were measured on samples polarized by 70 kV/mm and compared to samples poled 45kv/mm in this work, previous work and an analytical model. The surface morphology of samples was examined using a scanning electron microscope (SEM) and energy-dispersive X-ray spectroscopy (EDS).</p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head>Spin coat deposition speed and time profile study</head><p>The results from the spin coat speed and time interval studies are in Table <ref type="table">3</ref>. In Table <ref type="table">3</ref>, it is observed that the sample that was fabricated using Profile 1 had no piezoelectric response, which could be because the piezoelectric layer was so thin that there was not enough piezoelectric material in the layer to produce a readable piezoelectric response.</p><p>Samples fabricated using Profiles 2 and 3 demonstrated reasonable d 33 values that were &gt; 7 pC/N (the largest of the four profiles and datum). Samples fabricated using Profile 3 had a uniform thickness and highest value of d 33 <ref type="bibr">(7.</ref>52 pC/N).</p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head>Sol gel deposition layer study</head><p>The deposition study (over in Table <ref type="table">4</ref>) was done on 0.40 vol fraction of PZT. There were three starting viscosities, 150mPas, 248.7mPas and 299mPas respectively for this study, with 8 processes (A, B, C -G) including the datum study. As shown in Table <ref type="table">4</ref>, the sample fabricated with the datum process had no piezoelectric response, and neither do samples fabricated using process A, which had elevated viscosities in comparison to the datum. In the datum and Process A, samples that were thinnest had relatively low viscosity &lt; 299mPas. The low volume fraction of PZT deposited on the substrate during the deposition process, could be the cause of negligible piezoelectric response. Moreover, poling voltage was calculated based on the thickness of piezoelectric layer, which meant that low corona poling voltage could also lead to insufficient polarization.</p><p>Processes B, C and D incorporated two deposition layers. Samples that utilized the viscosity less than 249 mPas described for Process B expressed no piezoelectricity. Samples that were layered with an initial viscosity of 299mPas (Process B and C) had d 33 values &gt; 4.3 pC/N, i.e. 4.32 and 5.6 pC/N for Process B and C, respectively. Samples that were fabricated using Process C were polarized at a voltage of 45 kV/mm. Samples that were fabricated using the same process, but with lower viscosity had no piezoelectric response. Samples that were fabricated using Process D (higher viscosities, i.e. 248.7mPas and 299mPas) presented higher piezoelectric values. These samples experienced longer wait times prior to deposition of layers as detailed in Table <ref type="table">4</ref>, which could have enabled higher amounts of PZT particles to be included within the samples thickness. Samples fabricated using Processes E and F incorporated three layers of deposition as shown in Table <ref type="table">4</ref>. All samples fabricated using Process E demonstrated d33 values regardless of the initial viscosity employed. However, these samples incorporated longer wait times, (29 min detailed in Fig. <ref type="figure">5</ref>), prior to the deposition of electroactive layers. All of the samples fabricated using process F experienced dielectric break down during the poling process, though the initial viscosity was comparable to that used for Process E. The number of electroactive layers and presence of air gaps between layers resulting in contact resistance may have enhanced the probability of dielectric breakdown not evidenced in samples fabricated using Process B, C and D. All these studies show that consistent and fairly high piezoelectric coefficients could be achieved with samples of low volume fraction, i.e. 10-40% PZT however, multiple deposition layers at specific viscosities are required in order for a favorable thickness to be realized. Also, variation in layer thickness can be minimized when the deposition viscosity is increased to 300mPas-350mPas or when the viscosity is maintained in 150-300 mPa s and Profile E is employed.</p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head>Summary of optimized processing conditions</head><p>An overview of the data captured from samples where optimized processing conditions obtained from studies mentioned above are detailed in this section. Spin/Speed Profile 3 (detailed in Fig. <ref type="figure">4</ref>) rendered the highest d33 values regardless of PZT vf and deposition layer process. Samples fabricated using corona polarization produced higher d 33 coefficients than contact polarization.</p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head>PZT-epoxy domeoptimized fabrication method</head><p>In this section, a comprehensive summary of results from the optimization processes presented in Section 2 for PZT vfs ranging from 0.10 to 0.70. Corona polarization at 45kv/mm was used and the viscosity of the sol gel prior to the deposition of the first layer was maintained between 150 to 250 mPas. Samples with vfs &gt; 0.40 PZT were fabricated using Spin/Speed Profile 3 (Fig. <ref type="figure">4</ref>) and datum process (Fig. <ref type="figure">2</ref>), while samples with vfs &lt; 0.40 PZT were fabricated using Spin/Speed Profile 3 (Fig. <ref type="figure">4</ref>) and Process D (Fig. <ref type="figure">5</ref>).</p><p>It was found that samples that were less than 0.50 vol fraction of PZT were&#8764;39 &#956;m thinner than the samples with higher PZT vfs, which may be due to the ability of more sol to adhere to the surface of more PZT particles of higher volume fractions and the faster cure rate observed for high volume fractions. In addition, at high vfs of PZT, i.e. 0.6 and 0.7, the agglomerated PZT filler decreased the mobility of other PZT particles due to particle collisions <ref type="bibr">[38]</ref>, where these collisions dominate the immobilization of particles instead of the shear stress provided by epoxy.</p><p>The d 33 values for this work (with and without electrodes), from <ref type="bibr">[22]</ref> and predicted by Furukawa's analytical model <ref type="bibr">[36]</ref> are shown in Fig. <ref type="figure">6</ref>. Similar to the trends observed by Furukawa et al. <ref type="bibr">[36]</ref> and Seema et al. <ref type="bibr">[39]</ref>, the d 33 values increase with the volume fractions of PZT. For example, B. Satish et al. <ref type="bibr">[40]</ref> fabricated PZT-PVDF 0-3 composites and found that the piezoelectric coefficient expressed a positive correlation with the increasing volume fractions of PZT, which was also found by <ref type="bibr">[22]</ref>, where PZT bulk samples and thick films were fabricated and measured. The values they presented are comparable with our results which are 11.106 pC/N @70% volume fraction of PZT. However, some of our results are less than others (Satish et al. <ref type="bibr">[40]</ref> reported d 33 &#8764;28 pC/N) because our matrix material in electrically inactive, while others integrated PVDF as a matrix material, which has piezoelectric proper ies. The d 33 values from this work are one magnitude higher than the values obtained from previous work <ref type="bibr">[22]</ref> for several reasons. First, the sonication time was increased, which resulted in better dispersion of PZT particles and the Corona polarization technique allowed to the use of higher polarization voltages, which improved the efficacy of the polarization process. Modification of the layering of electroactive films enabled better properties for lower volume fractions.</p><p>The experimental values obtained in the present work agree with theoretical values (provided in Fig. <ref type="figure">6</ref>). For higher volume fractions of PZT, the experimental values are higher than predicted values by Furukawa et al. <ref type="bibr">[36,</ref><ref type="bibr">37]</ref>, because Furukawa's model assumes a uniform distribution and perfectly spherical filler, however the PZT filler used varies from 1 to 10 &#956;m with shapes varying from spherical to ellipsoid. At high volume fractions the PZT agglomeration occurs, which make the local electric fields around the filler higher than the theoretical values leading to higher piezoelectric responses. The transverse piezoelectric coefficients -d 31 values of this work and previous work are shown in Fig. <ref type="figure">7</ref>. The values of our present work are comparable to others, e.g. Furukawa et al. <ref type="bibr">[36,</ref><ref type="bibr">37]</ref>, wherein they produced PZT-PVDF 0-3 composites with 0.21 vol fraction PZT that piezoelectric strain coefficients equal to 4 pC/N. The piezoelectric strain coefficients are also comparable to samples that were thicker in geometry and fabricated with PZT powder with larger mean diameter size such as <ref type="bibr">[41]</ref> (d 33 = 18 pC/N and 1 mm thickness, and 50% vf), <ref type="bibr">[42]</ref>(d 33 = 13 pC/ N, 13.8 pC/N, 14 pC/N for PZT/PVC, PZT/PVDF and PZT/PVDF samples respectively <ref type="bibr">[42,</ref><ref type="bibr">43]</ref>. In addition, the piezoelectric strain values are higher than others of similar composition at comparable volume fractions <ref type="bibr">[31,</ref><ref type="bibr">44]</ref>. These results indicate that piezoelectric strain coefficients are influenced by several factors: the enhanced polarization field achieved via the Corona technique versus contact method, 2) reduction in PZT agglomeration via processing technique; and 3) dome-shaped geometrical structure of the sample that allows for better actuation response for applied loading conditions.</p><p>Capacitance was measured at room temperature @110 Hz, and the dielectric constant was calculated using Eq. 1. In both the previous work <ref type="bibr">[22]</ref> and this work, the dielectric constants increased with the volume fractions of PZT. The dielectric constant of this work are slightly smaller than previous work <ref type="bibr">[22]</ref> because of the reduction in agglomerated PZT and the associated surface charge and contact resistance, which promote higher capacitive storage. It is believed that ionic and electronic polarization mechanisms contributed to most to the higher dielectric constant values observed in this work. The agglomerations could be treated as effective larger particles, and the large particles could lead to higher dielectric constants as the interaction force between parties leads to the distortions toward more tetragonality <ref type="bibr">[45]</ref>.</p><p>As in Fig. <ref type="figure">6</ref>, the experimental values and the predicted values have similar trends, and experimental values and predicted values are comparable. In Table <ref type="table">5</ref>, a comparison of our previous work <ref type="bibr">[22]</ref> and this present work for 0.7 vf of PZT is presented Fig. <ref type="figure">8</ref>. In Fig. <ref type="figure">9</ref>, the d33/d31 for samples polarized at 70kv/mm (which could only be achieved at lower PZT volume fractions less than 0.40) are higher than samples poled with 45kv/mm. The d 33 captured from samples poled at 70kv/mm are more in agreement with the predicated values than samples poled at 45kv/mm shown in Fig. <ref type="figure">6</ref>. Transverse piezoelectric strain, d 31 values are similar regardless of polarization technique, but Corona poled samples have higher d 31 values than contact polarized samples. These results indicate that the corona polarization technique is more effective than the contact polarization method for piezoelectric 0-3 composites, such as these. This can be seen by the enhanced values of dielectric constant, &#949;, and the strain coefficients d 33 and d 31 for all volume fractions. The increase in the strain coefficients is due to the increase in effectiveness of the polarization process. The dielectric constant, which is measured in the 33-direction is also enhanced due to the increase in the number of the dipoles aligned along the 33-direction.</p><p>In Fig. <ref type="figure">10</ref>, the dielectric constants from our previous work and this present work are plotted as a function of the frequency range, dielectric constants increase as a function of vf of PZT. Space charge polarization is mostly responsible for the lower frequencies, while the values for the higher frequencies are most likely due to the effects of dipolar, ionic and electronic polarizations, since space charge polarizations do not present well at the higher frequencies. Within 1MHz&#8764;10 MHz frequency range, the dielectric constant is mostly the result of ionic and electronic mechanisms since both the space charge polarization and dipolar polarization could not follow the change of the external electric fields. The increasing dielectric constant with frequency above 10 MHz could be from the epoxy phase. The dielectric constant of present work is slightly smaller (43.7-68.1) than others of similar composition (PZT/ PVC, PZT/PVDF, PZT/epoxy) <ref type="bibr">[31,</ref><ref type="bibr">42,</ref><ref type="bibr">43,</ref><ref type="bibr">46]</ref>; this could also be because of the reduction of the sample thickness, as there was less dielectric material and smaller mean diameters of the PZT embedded in the matrix material.</p><p>The dissipation factors are depicted in Fig. <ref type="figure">11</ref>, and increase with the vf of PZT. The dissipation factor of PZT (&#8764;2.5%) is higher than the epoxy matrix (0.002&#8764;0.004). The spectrums show a substantial increase with the frequency, as epoxy's dissipation factor is relatively stable, so the increase is due to PZT. The dissipation factors of this work are smaller than previous work <ref type="bibr">[22]</ref>, due to the reduction of trapped air in the samples and better distribution of PZT. Space charge polarization occurs on the interface between the air pockets and composites material. This polarization induces the formation of two charge layers at the interfaces, however, this form of polarization cannot always be achieved at higher frequencies, in which case, the energy is dissipated as heat, resulting in higher dissipation factors.</p><p>In Fig. <ref type="figure">12</ref>, the impedance in our present and previous works decreases with the vf of PZT, while the impedance of the present work are significantly lower than our previous work, due to the reduction in agglomerated PZT particles and reduced air gaps. Under the influence of an electric field the dissolved free ions tend to move towards the electrode/epoxy interface, leading to the development of ionic double layers in such regions, which is called space charge polarization <ref type="bibr">[47]</ref>. This phenomenon could largely affect the measured resistant spectra.</p><p>In Fig. <ref type="figure">13</ref>, in both our previous and present work, the phase angles increase with frequency, which is due to the response of the material, which is different than a pure capacitive circuit, where the phase of the voltage is 90&#176;behind the alternating current. The increase in phase   angle with frequency is because the material is less dielectric at higher frequencies. The phase angle also increases as the volume fraction of PZT increases. In the present work, the phase angles for each volume fraction are lower than the values from our previous work, which could indicate that the updated method of fabrication leads to samples with better capacitive properties.</p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head>Surface morphology and PZT dispersion within the matrix</head><p>The mean and median diameter of PZT particles and clusters were characterized via SEM micrograph images and analysis software was   used to perform particle distribution analysis, as shown in Fig. <ref type="figure">14</ref>. Fig. <ref type="figure">15</ref> depict the surface morphology of 50%PZT and 60%PZT composites. The distribution plot shown in Fig. <ref type="figure">14</ref> indicates that the average particle size and median PZT particle diameter are 0.974 and 1.00 &#956;m, respectively. The surface morphology of the domed-shaped PZT-epoxy composite are observed with the aid of SEM images shown in Fig. <ref type="figure">15</ref> for samples of 50% and 60% volume fraction of PZT. These images indicate similar PZT cluster sizes with some aggregated PZT clusters in Fig. <ref type="figure">14</ref>. There are small porous regions shown for the 50% PZT volume fraction (Fig. <ref type="figure">15 A</ref>)). On the otherhand, the samples with    <ref type="figure">14</ref>. A) SEM micrograph images of pristine PZT particles/clusters and B) particle distributions used to determine the mean (average) and median particle/cluster sizes, which were 1.00 and 0.974 &#956;m respectively. the higher volume fraction (v f = 60%)of PZT is denser with less porosity. EDS micrograph images were taken for samples comprising 50% and 6-% volume fraction of PZT and are depcited in Figs. <ref type="figure">16</ref> and<ref type="figure">17</ref>, respectively. These images illustrate the distribution of PZT in the epoxy matrix. From the images in Fig. <ref type="figure">17</ref>, there PZT apppears to be well-distributed throughout the matrix, however, the porosity of the sample is higher than that of the 60% volume fraction samples. Reduction in pores shown in Fig. <ref type="figure">17</ref>, could lead to more effective polarization. The distribution of particles and sample porpsity is better than those of previous work <ref type="bibr">[31]</ref>, and enhancement of polarization due to reduced porosity and better PZT distribution are evidenced by higher values in piezoelectric strain coefficiencts than <ref type="bibr">[31]</ref>.</p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head>Conclusions</head><p>Novel PZT-epoxy composite thick films were fabricated using an optimized combination solvent and spin coat deposition technique for the synthesis of dome-shapes actuators. Parametric studies were performed to achieve the optimal fabrication procedure according to volume fraction of PZT. The surface and morphology were examined via  SEM and EDS. The piezoelectric coefficients, Capacitance and effective dielectric coefficient increased with the volume fraction of PZT. Also, the processing parameters such as spin-speed/time profiles and depositing techniques influenced the piezoelectric and dielectric properties of the dome-shaped devices. In particular, the piezoelectric strain coefficients in this work increased by a factor of 10 via use of the Corona polarization. Also, the piezoelectric strain coefficients of this work increased by a factor of 20 in comparison with our previous work in the design of dome-shaped 0-3 composite actuators. In addition, the dissipation factor associated with dielectric losses for this work decreased by nearly half. These results indicate that devices such as these may have potential for applications such as sensor, actuator, capacitor and low-power energy harvesting. </p></div></body>
		</text>
</TEI>