<?xml-model href='http://www.tei-c.org/release/xml/tei/custom/schema/relaxng/tei_all.rng' schematypens='http://relaxng.org/ns/structure/1.0'?><TEI xmlns="http://www.tei-c.org/ns/1.0">
	<teiHeader>
		<fileDesc>
			<titleStmt><title level='a'>Effect of recycled swarf and spherical Ti-6Al-4V feedstocks on laser directed energy deposition additive manufacturing</title></titleStmt>
			<publicationStmt>
				<publisher>CIRP</publisher>
				<date>01/01/2024</date>
			</publicationStmt>
			<sourceDesc>
				<bibl> 
					<idno type="par_id">10527112</idno>
					<idno type="doi">10.1016/j.cirp.2024.03.013</idno>
					<title level='j'>CIRP Annals</title>
<idno>0007-8506</idno>
<biblScope unit="volume">73</biblScope>
<biblScope unit="issue">1</biblScope>					

					<author>Sarah Wolff</author><author>Marwan Haddad</author><author>Jianyue Zhang</author><author>Alan Luo</author>
				</bibl>
			</sourceDesc>
		</fileDesc>
		<profileDesc>
			<abstract><ab><![CDATA[Feedstock from locally-sourced, recycled Ti-6Al-4V (Ti64) swarf is a low-cost alternative to atomized powder and encourages circular additive manufacturing. This study investigates the feasibility of Ti64 swarf as feedstock for laser directed energy deposition (L-DED) additive manufacturing. Ti64 swarf was recycled and ball-milled into irregular-shaped powder and compared to spherical plasma-atomized powder in powder flow, melt flow, and resulting microstructure. In situ monitoring showed that plasma-atomized powder had laminar flow during deposition and that ball-milled swarf powder had turbulent flow. Plasma-atomized powder had steady melt pool dynamics and acicular microstructure. Ball-milled swarf powder caused melt pool fluctuation and equiaxed microstructure.]]></ab></abstract>
		</profileDesc>
	</teiHeader>
	<text><body xmlns="http://www.tei-c.org/ns/1.0" xmlns:xsi="http://www.w3.org/2001/XMLSchema-instance" xmlns:xlink="http://www.w3.org/1999/xlink">
<div xmlns="http://www.tei-c.org/ns/1.0"><head n="1.">Introduction</head><p>Ti-6Al-4V (Ti64) is a titanium alloy with a high strength-toweight ratio used widely for transportation, aerospace, and biomedical applications. Additive manufacturing (AM) of Ti64 components has increased in demand recently due to design flexibility, geometric complexity, and feedstock material savings compared to conventional processing that entails multiple steps of joining and subtractive manufacturing. However, many metal AM processes require plasma or gas-atomized powder feedstock that are costly and energy intensive <ref type="bibr">[1]</ref>. A feedstock alternative is Ti64 swarf, or discarded material from industrial scale production of Ti64 fabrication. Due to the high cost of Ti64 fabrication, recycling Ti64 has gained attention, with Ti64 swarf, or scrap, as a major source for high-efficiency recycling <ref type="bibr">[2]</ref>. Therefore, this study explores Ti64 swarf as a feedstock material for metal AM processes such as Laser Directed Energy Deposition (L-DED), a possible application of industrial symbiosis <ref type="bibr">[3,</ref><ref type="bibr">4]</ref>.</p><p>L-DED is an AM process that deposits powder feedstock into a melt pool created by a laser source to manufacture a part by subsequent printed layers <ref type="bibr">[5]</ref>. Previous work investigated the feasibility of recycling metal swarf for L-DED processes. For example, <ref type="bibr">Mahmood et al.</ref> showed the feasibility of reducing material usage by printing with carbon steel chips <ref type="bibr">[5]</ref>. Fullenwider et al. recycled 304 L stainless steel machining chips into feedstock powder and successfully printed single layer tracks with L-DED, resulting in melt tracks with similar morphology to those printed with gas-atomized powder <ref type="bibr">[6]</ref>. Jackson et al. compared 316L parts from L-DED gas-atomized powder and those from mechanically generated feedstock, finding that their microstructure, surface texture, and most mechanical properties were similar, with an increase in tensile strength for parts from mechanically generated feedstock <ref type="bibr">[7]</ref>. <ref type="bibr">Murray et al.</ref> found that chips that were not cleaned from cutting fluid residue were viable feedstock for the L-DED process <ref type="bibr">[8]</ref>.</p><p>Relative to the literature, the novelty of the presented work is in (Fig. <ref type="figure">1</ref>): (1) In situ and ex situ comparison analysis, before, during, and after printing, between plasma-atomized (PA) Ti64 powder and ball-milled (BM) Ti64 swarf powder and (2) L-DED printing of PA Ti64 powder and BM Ti64 swarf to compare results from both powder feedstocks. Overall, the findings show the viability of recycled Ti64 swarf powder as an alternative feedstock for L-DED processes. Captured in situ high-speed images suggest that process dynamics differ between the different powder and their outcomes. </p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head>Contents lists available at SciVerse ScienceDirect</head></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head>CIRP Annals Manufacturing Technology</head><p>Journal homepage: <ref type="url">www.elsevier.com/locate/cirp</ref> </p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head n="2.">Material and methods</head><p>This study concerns two types of feedstocks for the L-DED process: PA Ti64 powder and recycled, BM Ti64 swarf powder. The Ti64 PA powder was from AP&amp;C Powder Metallurgy (GE Additive -Canada) with a size distribution between 45-106 &#956;m. The Ti64 swarf (Fig. <ref type="figure">2</ref>) was collected from a local metal scrap recycling facility (Stargate Metals -Columbus, OH, USA), ranging in size from 5 to 25 mm in width. The swarf represented material from cutting operations, as observed by the swarf morphology in Fig. <ref type="figure">2</ref>. Most of the swarf were segmented machining chips, or serrated, with 6s and 9s shapes with a smooth side and a serrated side (see Supplementary Material). The swarf was then BM for 6 hours with 10 mm diameters stainless steel balls at 600 rpm. There was no cleaning before or after ball milling because most impurities from machining coolant evaporates during the L-DED process <ref type="bibr">[8]</ref>. Subsequently, a vibratory sieve shake sieved the powder with 100 and 325 meshes for 2 hours to achieve a particle size distribution between 43 and 150 for optimal L-DED deposition <ref type="bibr">[9]</ref>. Finally, the BM powder was in a vacuum drying oven at 423 K for 24 hours to remove moisture.</p><p>The printing occurred in an in-house custom L-DED glovebox system with a 3-axis motorized stage, consisting of a single nozzle with a hopper (20 mL) designed for small quantity testing and an ytterbium fiber laser head with a 400 W maximum power. During printing, the laser diameter was 2 mm and offset above the focal plane by 30 mm. An off-axis high speed camera (FASTCAM SA-Z-Photron Japan) captured real-time images from outside the glovebox. Energy Dispersive X-Ray Analysis (EDX) measured the powder composition. X-ray diffraction (XRD) analysis detected the phases in the powder. Lastly, Optical Microscope (OM) and Apreo I (FEI Apreo LoVac Analytical) high resolution scanning electrical microscope (SEM) revealed the final parts' microstructures. </p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head n="3.">Results and discussion</head></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head n="3.1.">Powder characteristics</head><p>Figures <ref type="figure">3a</ref> and <ref type="figure">b</ref> are SEM images of PA and BM powder. BM powder particles (Fig. <ref type="figure">3b</ref>) have irregular shapes and sizes compared to the spherical shapes of the PA powder particles (Fig. <ref type="figure">3a</ref>). In addition, BM powder included small irregular shaped particles with a smaller size distribution than that of PA powder. The distributions of the effective diameter (see supplementary materials) for both powder types are in the boxplots in Fig. <ref type="figure">3c</ref>. The BM powder particles have a lower average effective diameter (around 40 &#181;m) than that of the PA powder (around 55 &#181;m), and a lower first quartile (around 29 &#181;m for BM powder and 50 &#181;m for PA powder). Although the average effective diameter size of the BM powder is close to the 325-mesh opening size (43 &#181;m), a sizable portion (25 %) of BM powder is smaller than 29 &#181;m, compared with PA powder, where most of the effective diameters are above 50 &#181;m.</p><p>Meanwhile, multiple EDX measurements of BM powder do not show impurities such oxygen or residue from machining lubricants. XRD scans displayed in Fig. <ref type="figure">3d</ref> show that the peak patterns for both materials match approximately and align with (hkl) values of the Ti Hexagonal Close-Packed (HCP) &#945; phase <ref type="bibr">[10]</ref>. However, BM powder's XRD patterns exhibit a slight difference in peak intensity and width with a shift to the left, which can be correlated to the crystallite size and presence of micro-strains from the ball milling process <ref type="bibr">[11,</ref><ref type="bibr">12]</ref>. </p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head n="3.2.">Powder flow</head><p>To clearly see the powder flow during printing, the laser was OFF, and the argon carrier gas had a pressure of 34.5 kPa. The mass flow rates for BM and PA powder were 15.10 -3 g/s and 42.10 -3 g/s, respectively. The difference in flow rates is due to both the irregular shape of the BA powder and greater distribution of very small particles in the BA (&lt;30 &#181;m), even after sieving. High-speed images were captured at 10,000 fps with a field of view (FOV) of 15 mm x 15 mm (1024 x 1024 pixels) and a pixel size of 20 &#956;m.</p><p>The images show the trajectory of the powder particles deposited from the nozzle until impact with the Ti64 substrate. Rendered recordings of the high-speed images are in Supplementary Videos S1 and S2. For PA powder in Supplementary Video S1, the argon gas flow was laminar, and the kinetic energy of the powder particles did not decrease after impact with the substrate as the speed before and after impact was around 3.3 m/s. Figure <ref type="figure">4a</ref> displays the traced trajectory of a PA powder particle characterized by a straight line.</p><p>As for the BM powder flow in Supplementary Video S2 and Fig. <ref type="figure">4b</ref>, the flow is laminar when particles exit the nozzle, and then transitions (white horizontal dashed line) to turbulent flow before impact with the underlying Ti64 substrate. Furthermore, the traced trajectory of the BM powder particle (yellow arrow lines) diverges away from the trajectory of the center axis of the nozzle (red dashed line), opposed to the straight-line trajectory of the traced PA powder particle in Fig. <ref type="figure">4a</ref>. Moreover, a turbulent vortex materializes behind the BM powder stream after impact with the substrate surface. Moreover, there is loss of kinetic energy as the measured speed before and after impact was around 3.4 m/s and 0.8 m/s, respectively. Figure <ref type="figure">4</ref>.b shows the traced trajectory of an irregular BM powder particle, the laminar gas flow near the nozzle, the turbulent flow above the substrate, and the vortex behind the flow. In addition, the BM powder flow is denser than the PA powder flow even though the mass flow rate of BM powder is smaller. The occurrence of the turbulent flow, the vortex, and the dense flow is because of the irregular shape of the BM powder and the existence of a significant amount of small powder particles in the BM powder interacting with the argon gas flow. </p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head n="3.3.">Printing with L-DED</head><p>L-DED printing for both powder feedstocks occurred in an inert environment (&lt;100 ppm oxygen concentration). The printing parameters for both powders were 276 W laser powder and 4 mm/s scanning speed. High-speed images were captured at 10,000 fps with a FOV of 14 x 14 mm (1024 x 1024 pixels) and 20 &#956;m/pixel resolution. Supplementary Videos S3 and S4 show the printing, or laser melting, of a single layer of 3mm length with PA powder and BM powder on a Ti64 substrate. The videos show the onset of melting, a molten pool in steady-state, and solidification at the end of a print. The supplementary videos show how both deposited layers for PA and BM powder are continuous, without balling, and similar in geometry to each other. However, powder particles from the PA and BM feedstock interact differently with the melt pool.</p><p>In Supplementary Video S3, the molten pool is steady during printing. A portion of the PA powder floats on the top of the surface of the molten melt pool for an interval of time before submerging into the liquid metal. This phenomenon was also recorded in a previous work by Haley et al. on L-DED with 316L spherical gas atomized feedstock <ref type="bibr">[13]</ref>. Additionally, bright spots (largest measured area 0.1 mm 2 ) emerged on the surface of the molten metal as surface pores, which can increase in size, coalesce, explode, or solidify resulting in a rough surface of the track as reported by Zhang et al. <ref type="bibr">[14]</ref>. Figure <ref type="figure">5a</ref>  In Supplementary Video S4, during the deposition of BM powder, the surface of the melt pool fluctuates at a rate faster than the 0.1 ms time interval between frames, with apparent surface ripples. Contrary to PA powder, BM powder particles do not float on top of the molten surface. However, large bright white spots (largest measured area 0.15 mm 2 ) are on the melt pool surface, which lead to large pores and a rough solidified surface.</p><p>Figure <ref type="figure">6</ref> illustrates the fluctuation and rippling of the melt pool surface and the non-presence of floating particles for BM powder deposition. At the start of the image sequence (Fig. <ref type="figure">6a</ref>), a BM powder particle collides with the surface of the melt pool, which induces splashing of the liquid metal and the formation of a bright spot on the melt pool surface. Then in Fig. <ref type="figure">6b</ref>, after a time interval of 0.1 ms (one frame), the molten liquid engulfs the powder particles. Thus, the shape of the BM powder may be a factor in the interaction of BM powder particles with the argon carrier gas and the molten pool. This interaction causes splashes that subsume the powder particles into the molten pool, generating high frequency ripples on the surface. Another cause for fluctuations is the turbulent flow and vortex of the BM powder flow, discussed in the powder flow analysis section and observed above the melt pool in Supplementary Video S4, which induces vibration at the top surface of the molten metal. Figure <ref type="figure">6c</ref> is a representation of the L-DED process when BM powder deposits into the melt pool, displaying the ripples and the formation of large bright spots when the irregular powder particle penetrates the melt pool surface. </p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head n="3.4.">Microstructure</head><p>Two one-layer samples with a length of 10 mm were printed with the same input parameters and showcased the same melt pool phenomena as those used and observed in the previous section. After printing, the cross-sections of the two samples were polished and immersed in a Kroll's reagent solution. Using OM and SEM, the microstructures were analyzed.</p><p>For the sample printed with PA powder, there are no pores in the cross-section (Fig. <ref type="figure">7a</ref>) and there is an acicular (needle-like) microstructure in Fig. <ref type="figure">7b</ref>, indicating martensitic transformation caused by the rapid cooling rate of the melt pool <ref type="bibr">[15]</ref>. The observed microstructure is consistent with the large mass flow rate of the PA powder into the melt pool, which causes a rapid cooling rate. A larger mass flow rates attenuates the laser beam and absorbs more laser energy away from the substrate, prompting a smaller melt pool (0.7 mm in length) and a rapid cooling rate.</p><p>Alternatively, the cross-section of the BM powder sample reveals pores with varying sizes (Fig. <ref type="figure">7c</ref>) and an equiaxed fine grain microstructure (Fig. <ref type="figure">7d</ref>). Factors for the formation of porosity and fine grain microstructure are the irregular shape and chemical composition of the BM powder, the interactions among the irregular powder particles, the molten pool, and the argon gas, the lower mass flow rate, along with the turbulent flow of the powder flow. First, the formation of pores is from the entrapment of argon gas by the irregular shape of the powder inside the melt pool . Because the swarf is not cleaned of machining coolant before the additive manufacturing process, an additional source of pores is the release of undetected impurities from coolant upon vaporization inside the melt pool.. Lastly, the existence of large pores is due to the pore coalescence mechanism of smaller pores into larger ones. Similar dynamics were observed for hydridedihydride (HDH) irregular Ti64 powder in L-DED using X-ray high speed imaging by Wang et al. and Haddad et al. <ref type="bibr">[16,</ref><ref type="bibr">17]</ref>. Second, the smaller mass flow rate of the BM powder moderately attenuates the laser beam which leads to a bigger absorption of laser energy into the substrate. The additional heating creates a large melt pool (1 mm in length). With a larger melt pool, the cooling rate is slower during solidification, and the martensitic phase transformation is unachievable. Third, these interactions and powder flow induced fluctuations that may function as sources of high frequency vibration in the liquid metal. The high-intensity vibration of molten pool results in the formation of cavitation and consequent implosion of cavities. Therefore, the resulting intensive shock waves refine Ti64 grain nucleation and forms equiaxed grains in samples produced with BM powder. Ultrasonic vibration techniques in molten metal alloys lead to similar grain refinement mechanisms <ref type="bibr">[18]</ref>. </p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head n="4.">Conclusions</head><p>In this work, recycled Ti64 swarf was ball milled into powder feedstock and compared with Ti64 plasma-atomized feedstock for L-DED process applications. In situ with ex situ analysis led to the following conclusions: Overall, this work shows the feasibility of recycled Ti64 swarf as feedstock for L-DED additive manufacturing, with the understanding that different microstructures result based on feedstock selection. Future work will focus on employing other in situ methods to further study the behavior of BM powder recycled from Ti64 swarf during the L-DED process.</p></div></body>