			<titleStmt><title level='a'>Room temperature polar and weak-ferromagnetic oxide with low dielectric loss</title></titleStmt>
			<publicationStmt>
				<publisher>Elsevier</publisher>
				<date>12/01/2023</date>
			</publicationStmt>
			<sourceDesc>
				<bibl> 
					<idno type="par_id">10559929</idno>
					<idno type="doi">10.1016/j.mseb.2023.116869</idno>
					<title level='j'>Materials Science and Engineering: B</title>
<idno>0921-5107</idno>
<biblScope unit="volume">298</biblScope>
<biblScope unit="issue">C</biblScope>					

					<author>Nagamalleswari Katragadda</author><author>Pranab Mandal</author><author>Premakumar Yanda</author><author>A Sundaresan</author><author>SD Kaushik</author><author>Weiguo Zhang</author><author>P Shiv Halasyamani</author><author>Alicia María Manjón-Sanz</author>
				</bibl>
			</sourceDesc>
		</fileDesc>
		<profileDesc>
			<abstract><ab><![CDATA[Single-phase materials that are simultaneously ferroelectric and ferromagnetic at room temperature are promising for devices such as non-volatile random-access memory. Perovskite BiFeO 3 which crystallizes in the polar rhombohedral structure (R3c) is ferroelectric and antiferromagnetic at room temperature. Here, we report a family of perovskite oxides in the BiFeO 3 -Bi 2/3 TiO 3 -ATiO 3 (where A 2+ is divalent alkaline earth metal ions e. g., Ca 2+ , Sr 2+ , Ba 2+ ) ternary phase diagram that is polar as well as weak ferromagnetic above room temperature. The composition (Bi 0.9167 A 0.075 )(Fe 0.9 Ti 0.1 )O 3 crystallizes in the polar rhombohedral structure space group R3c as corroborated by powder X-ray and neutron diffraction analysis. The nearly pure A-site perovskite possesses a long-range magnetic ordering above room temperature. These perovskites show a low dielectric loss, and the electrical response is dominated by grain contributions below 723 K.]]></ab></abstract>
		</profileDesc>
	</teiHeader>
	<text><body xmlns="http://www.tei-c.org/ns/1.0" xmlns:xsi="http://www.w3.org/2001/XMLSchema-instance" xmlns:xlink="http://www.w3.org/1999/xlink">
<div xmlns="http://www.tei-c.org/ns/1.0"><head n="1.">Introduction</head><p>Bismuth-based perovskite oxides (BiMO 3 , where M 3+ is a transition metal ion) are promising due to their versatile properties such as Pb-free piezoelectrics, multiferroics, solar cells etc <ref type="bibr">[1]</ref><ref type="bibr">[2]</ref><ref type="bibr">[3]</ref><ref type="bibr">[4]</ref><ref type="bibr">[5]</ref>. Especially pure A-site bismuth-based perovskite oxides that possess a polar structure are candidates for Pb-free piezoceramics. Among these, only a few perovskites, e.g., BiFeO 3 , BiTi 3/8 Fe 2/8 Mg 3/8 O 3, are accessible at ambient pressure <ref type="bibr">[6,</ref><ref type="bibr">7]</ref> whereas BiMnO 3 , BiInO 3 , BiNiO 3, and BiAlO 3 are high-pressure phases <ref type="bibr">[8]</ref><ref type="bibr">[9]</ref><ref type="bibr">[10]</ref>. BiFeO 3 has been extensively studied as a candidate material for room-temperature multiferroic <ref type="bibr">[3,</ref><ref type="bibr">[11]</ref><ref type="bibr">[12]</ref><ref type="bibr">[13]</ref>, and piezoceramics <ref type="bibr">[2,</ref><ref type="bibr">14]</ref> and has been demonstrated in random access memory device applications. At room temperature, the structure of BiFeO 3 is rhombohedral (space group R3c) with ferroelectric polarization along the [1 1 1] p direction. Ferroelectric switching has been reported in both ceramics and thin-film heterostructures with polarization as high as 60 &#956;C/cm 2 <ref type="bibr">[13,</ref><ref type="bibr">15]</ref>. The long-range G-type magnetic ordering in BiFeO 3 onsets below 675 K, however, the magnetic structure is modulated with a cycloidal ordering with a long period of 620 &#197; along the [1 1 0] h direction <ref type="bibr">[16]</ref>. This modulation cancels any net magnetization due to Dzyaloshinsky-Moriya interaction as commonly observed in rare-earth orthoferrites. Epitaxial strain, chemical substitution at the A-site or Bsite by Ti, and pressure has been shown to improve the magnetization in BiFeO 3 <ref type="bibr">[12,</ref><ref type="bibr">14,</ref><ref type="bibr">[17]</ref><ref type="bibr">[18]</ref><ref type="bibr">[19]</ref><ref type="bibr">[20]</ref><ref type="bibr">[21]</ref><ref type="bibr">[22]</ref><ref type="bibr">[23]</ref><ref type="bibr">[24]</ref>. For example, the polar and weak ferromagnetic phase is sustained up to x = 0.11 in BiFe 1-x Ti x O 3+&#948; and up to x = 0.2 in Bi 1-x A x FeO 3 where A = La, Ca, Sr, Ba) <ref type="bibr">[25]</ref><ref type="bibr">[26]</ref><ref type="bibr">[27]</ref>. New design routes can lead to materials that are both ferroelectric and ferromagnetic above room temperature. For example, a bulk perovskite oxide exhibited both switchable polarization and magnetization from a design strategy that led to improved ferroelectric properties at the morphotropic phase boundary and a sustained long-range magnetic order from a percolating network of magnetic ions <ref type="bibr">[28,</ref><ref type="bibr">29]</ref>. Synthesis and ceramic processing of BiFeO 3 are known to be challenging due to its phase instability, competing secondary phases, bismuth volatility, and purity of starting oxides and precautions are necessary to overcome these challenges <ref type="bibr">[11,</ref><ref type="bibr">30,</ref><ref type="bibr">31]</ref>.</p><p>Rare earth orthoferrites, e.g., LaFeO 3 , have a perovskite structure where trivalent La and Fe occupy the A and B sites of the perovskite, respectively <ref type="bibr">[32]</ref>. There are only a few A-site deficient perovskites known in the literature, e.g., La 2/3 TiO 3, which accommodates cations of higher oxidation states at the B-site <ref type="bibr">[33,</ref><ref type="bibr">34]</ref>. It has been reported that the bismuth analog of La 2/3 TiO 3, i.e., Bi 2/3 TiO 3 <ref type="bibr">[35]</ref> , aids to improve the density and resistivity of PbTiO 3 ceramics <ref type="bibr">[36]</ref>. Here, we have studied the effect of Bi 2/3 TiO 3 substitution on the ferroelectric and magnetic properties of BiFeO 3 . The BiFeO 3 -Bi 2/3 TiO 3 solid solution avoids Bi 3+ dilution at the A-site and introduces Ti 4+ at the B-site. The lone pair effect of Bi 3+ at the A-site and second order Jahn-Teller effect due to the closed-shell (d 0 ) electronic configuration of Ti 4+ ion is expected to promote ferroelectricity in these perovskites <ref type="bibr">[37]</ref>. We find that the stability of the perovskite phase improves in the BiFeO 3 -Bi 2/3 TiO 3 -ATiO 3 ternary phase diagram where A 2+ = Ca 2+ , Sr 2+ , and Ba 2+ . The resulting perovskite oxides are simultaneously polar and weak ferromagnetic at room temperature with about 90% bismuth at the A-site.</p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head n="2.">Materials and methods</head><p>The compounds in the BiFeO 3 -Bi 2/3 TiO 3 -ATiO 3 (A 2+ = Ca 2+ , Sr 2+ , Ba 2+ ) were prepared by conventional solid-state route using high-purity starting materials; Bi 2 O 3 (&gt;99 % Loba Chemie), CaCO 3 (&gt;99 % Loba Chemie), SrCO 3 (&gt;99 % Loba Chemie), BaCO 3 (&gt;99 % Loba Chemie), TiO 2 (&gt;99 % Loba Chemie), and Fe 2 O 3 (&gt;95 % Loba Chemie). The details of the compositions prepared in this study are summarized in Tables <ref type="table">S1</ref> and <ref type="table">S2</ref>, Supporting information. The starting materials were preheated at 180 &#8226; C for 10 h to remove any moisture. The stoichiometric ratio of starting oxides and carbonates was mixed in an agate mortar pestle in acetone. The homogenized powders were calcined in an alumina crucible at 750 &#8226; C, 800 &#8226; C, and 850 &#8226; C for 12 h with intermittent grindings between heating. The phase pure powders were mixed with a binder (Polyvinyl butyral 2 wt%), pressed into pellets, and sintered at temperatures between 870 and 950 &#8226; C to obtain pellets above 90% of the crystallographic density. The phase purity and crystal structure were studied using powder X-ray diffraction (XRD) using CuK-&#945; radiation in a powder X-ray diffractometer (PANalytical Empyrean). Powder neutron diffraction (PND) experiments were carried out employing POWGEN diffractometer (Spallation Neutron Source at Oak Ridge National Laboratory) <ref type="bibr">[38]</ref> and PD3 multi PSD based focusing crystal diffractometer set up by UGC-DAE Consortium for Scientific Research Mumbai Centre at the National Facility for Neutron Beam Research (NFNBR), Dhruva reactor, Mumbai, India <ref type="bibr">[39]</ref>. For the experiment at POWGEN, around g of sample was placed in a 6 mm diameter vanadium can and loaded into the vacuum furnace. The data were collected at 300 K for 2 h. A central wavelength of 1.5 &#197; was used, covering a d-spacing of 0.5-10.85 &#197;. Structural analysis was carried out using software packages High-Score (XRD data), Fullprof <ref type="bibr">[40]</ref> (BARC data), and TOPAS-Academic POWGEN data) <ref type="bibr">[41]</ref>. Microstructure and composition were studied using a Hi-Resolution Scanning Electron Microscope (HRSEM) (Thermosceintific Apreo S). For dielectric and ferroelectric measurements, polished pellets of thickness 150-200 &#181;m were painted with silver paste and cured at 120 &#8226; C for 1 h. An LCR meter E4980A was utilized to evaluate dielectric properties in the frequency range between 100 Hz and 1 MHz. Complex impedance properties were measured using a custom-made furnace and impedance probe setup <ref type="bibr">[42]</ref>. The ferroelectric hysteresis loops were evaluated at room temperature by a Precision Multiferroic II Ferroelectric Test System (Radiant Technologies, Inc., USA). The Second harmonic generation (SHG) was measured by using a 1064 nm pulsed Nd: YAG laser (Quantel Laser, Ultra 50) to offer the fundamental light and the generated second harmonic light to be detected and monitored by an oscilloscope system (Tektronix, TDS3032). Samples were filled in fused silica tubes with an outer diameter of 4 mm. Relevant comparisons with known SHG material, &#945;-SiO 2 , were made at the same condition. The laser-generated fundamental light and the SHG intensity were recorded at room temperature on an oscilloscope <ref type="bibr">[43]</ref>. The DC magnetization data was collected in zero-field-cooled (ZFC) and field-cooled (FC) modes using a magnetic property measurement system (MPMS, Quantum Design, USA). For high-temperature magnetic data, the measurements were carried out in an oven option of the Physical property measurement system (PPMS, Quantum Design, USA).</p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head n="3.">Results and discussion</head></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head n="3.1.">Materials synthesis</head><p>Attempt to synthesize Bi 2/3 TiO 3 at 850 &#8226; C for 12 h resulted in various secondary phases (Bi 4 Ti 3 O 12 , Bi 8 Ti 16 O 44 ), and there was no indication of the perovskite phase (Fig. <ref type="figure">S1</ref>, Supporting Information). It should be noted that Bi-based perovskite e.g., BiMnO 3 , BiCrO 3 , BiAlO 3 , and BiInO are metastable phases that can only be stabilized by high-pressure synthesis. It is possible that Bi 2/3 TiO 3 could be a metastable phase and cannot be stabilized using the ambient pressure solid state route. Divalent alkaline earth metal ions (A 2+ = Ca 2+ , Sr 2+ , Ba 2+ ) were substituted at the Bi-site to stabilize Bi 2/3 TiO 3 in the perovskite phase in the range 0.1 &#8804; y &#8804; 0.5 in Bi 2/3-y A 3y/2 TiO 3 . The calculated tolerance factor Bi 2/ 3-y Ca 3y/2 TiO 3 is near the perovskite limit (0.95 -1.05) as shown in Table <ref type="table">S1</ref> (Supporting Information). The XRD patterns indicate secondary phases (Fig. <ref type="figure">S1</ref>, Supporting Information). These compositions are shown in the Bi 2/3 TiO 3 -CaTiO 3 line in the ternary phase diagram Fig. <ref type="figure">1a</ref>.</p><p>We then prepared (1-x)BiFeO 3 -xBi 2/3 TiO 3 using the solid-state route. Powder XRD patterns show that the compositions x = 0.9 and 0.7 were formed with secondary phases, with no indication of a perovskite phase (Fig. <ref type="figure">S2</ref>, Supporting Information). This is indicated as the brown squares in the Bi 2/3 TiO 3 -BiFeO 3 line (baseline of the triangle) in the ternary phase diagram (Fig. <ref type="figure">1a</ref>). For x = 0.5 and 0.3, a perovskite phase forms with other secondary phases as represented using filled red circles in the ternary phase diagram. The calculated tolerance factor of compositions in (1-x) BiFeO 3 -xBi 2/3 TiO 3 ranges from t = 0.84 to t = 0.95 for x = 0.7 to x = 0.1, respectively.</p><p>To tune the tolerance factor towards the perovskite range (~0.94 to 1.04), divalent alkaline earth metal ions were substituted at the Bi-site in the solid solution (1-x)BiFeO 3 -xBi 2/3-y A 3y/2 TiO 3 (A 2+ = Ca 2+ , Sr 2+ , Ba 2+ ) which can be represented in the ternary phase diagram of BiFeO 3 -Bi 2/3 TiO 3 -ATiO 3 (A 2+ = Ca 2+ shown in Fig. <ref type="figure">1a</ref>). As can be seen from Fig. <ref type="figure">1b</ref>, the introduction of divalent Ca 2+ has a significant effect on the phase purity. For x = 0.3, y = 0.1-0.5 (x = 0.3 dotted line), and x = 0.5, y = 0.1-0.5 (x = 0.5 dotted line) the phase purity improves; however, the perovskite phase forms with other impurities represented filled by red circles. For x = 0.1, y = 0.3, and x = 0.1, y = 0.5 phase pure perovskite forms as indicated by filled blue circles (x = 0.1, y = 0.5 shown as pattern 2 in Fig. <ref type="figure">1b</ref>). Ternary phase diagrams with A 2+ = Sr 2+ and Ba 2+ show similar trends as shown in Table <ref type="table">S2</ref> (Supporting Information). The compositions in the solid solution (1-x)BiFeO 3 -xBi 2/ 3-y A 3y/2 TiO 3 for A 2+ = Ca 2+ , Sr 2+, and Ba 2+ are represented as BCFTxy, BSFTxy, and BBFTxy respectively as summarized in Table <ref type="table">S1</ref> and Table <ref type="table">S2</ref>, Supporting Information. In this work, BCFT15 (x = 0.1, y = 0.5 for A 2+ = Ca 2+ ) and BSFT15 (x = 0.1, y = 0.5 for A 2+ = Sr 2+ ) have been Fig. <ref type="figure">2</ref>. (a) Profile fit to room-temperature powder X-ray diffraction data of BCFT15. Black points show the data, Red lines the fit, blue line the difference plot, and green markers show Bragg positions (b) A strong reflection near d ~ 4.56 &#197; in 300 K PND data (POWGEN) confirms longrange magnetic ordering; the blue arrow indicates the magnetic peaks (c) PND data at 800 K (POWGEN) showing absence magnetic peak consistent with magnetization data (Fig. <ref type="figure">3</ref>). Small amount of secondary phases indicated with * and^represents Bi 2 Fe 4 O 9 and unidentified impurity respectively. (For interpretation of the references to colour in this figure legend, the reader is referred to the web version of this article.) Fig. <ref type="figure">3</ref>. (a) Zero-field cooled (ZFC) and field cooled (FC) magnetization data of BCFT15 against temperature showing magnetic ordering at 557 K as calculated from the derivative of FC data (inset). (b) Magnetic isotherm at 300 K (black line) and 600 K (red line) of composition BCFT15 confirmed weak ferromagnetism at room temperature. (For interpretation of the references to colour in this figure legend, the reader is referred to the web version of this article.) studied in detail.</p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head n="3.2.">Structural analysis</head><p>Structural analysis was focused on the phase pure perovskite composition BCFT15. Profile fit to the laboratory X-ray data on BCFT15 confirms that all the reflections can be explained by the rhombohedral space group R3c. A small amount (&lt;2 %) of secondary phases was present (Fig. <ref type="figure">2</ref>). The refined lattice parameters obtained from the profile fit are a = 5.5670 (2) &#197;, c = 13.8034(2) &#197; and V = 370.47 &#197; 3 . The change in lattice parameters from the lattice parameters of BiFeO 3 (a = 5.579 &#197;, c = 13.869 &#197;, and V = 373.44 &#197; 3 ) suggests that a solid solution is formed. Preliminary Rietveld refinement suggests a reasonably fit to space group R3c and the structural parameters are provided in Fig. <ref type="figure">S4</ref> and Table <ref type="table">S3</ref>, Supporting Information. The reduction in cell parameters is due to the difference in the ionic radii of Bi 3+ (r = 1.17 &#197;), Ca 2+ (r = 1.34 &#197;), Fe 3+ (r = 0.645 &#197;), and Ti 4+ (r = 0.605 &#197;) <ref type="bibr">[7,</ref><ref type="bibr">31]</ref>. A similar trend has been observed in the solid solution of BiFeO 3 and CaTiO 3 <ref type="bibr">[30]</ref>. It is noteworthy, that in BiFeO 3 -CaTiO 3 , the polar rhombohedral structure (R3c) of BiFeO 3 extends up to x = 0.2, and above the limit, the structure changes to a non-polar orthorhombic structure with space group Pnma <ref type="bibr">[44]</ref>. The powder XRD patterns of compositions BAFT11 and BAFT13 for A 2+ = Ca 2+ , Sr 2+ , and Ba 2+ show a similar trend, and the patterns can be explained using the rhombohedral structure R3c (Table <ref type="table">S2</ref>, Supporting Information). Second harmonic generation (SHG) experiments were conducted on compositions BAFT13, BAFT15 for A 2+ = Ca 2+ , Sr 2+ , and Ba 2+ . All six compositions are found to be SHG active and corroborate with the polar or non-centrosymmetric structure <ref type="bibr">[43,</ref><ref type="bibr">45]</ref> (data shown in Fig. <ref type="figure">4b</ref> for BCFT15 and BSFT15). The SHG data for other compositions are shown in (Fig. <ref type="figure">S6</ref> Supporting Information). The SEM micrographs of the composition BCFT15, and BSFT15 show a typical grain-like feature with an average microparticle size of 1-2 &#956;m (Fig. <ref type="figure">S3</ref>, Supporting Information). The average compositions were calculated from energy-dispersive X-ray spectroscopy (EDX) measurements for BCFT15 and BSFT15 are (Bi 0.804 Ca 0.061 )(Fe 0.9 Ti 0.099 )O 3 and (Bi 0.740 Sr 0.059 )(Fe 0.9 Ti 0.077 )O 3 which are close to their target compositions (Bi 0.9167 Ca 0.075 )(Fe 0.9 Ti 0.1 )O 3 and (Bi 0.9167 Sr 0.075 )(Fe 0.9 Ti 0.1 )O 3 respectively. The profile fit, lattice parameter trend, and compositional analysis exclude the possibility of phase separation and therefore the SHG response is consistent with the polar structure with space group R3c.</p><p>The room temperature PND data of BCFT15 (Fig. <ref type="figure">2b</ref>) reveals a strong reflection at d ~ 4.56 &#197;. This reflection is not allowed in the rhombohedral space group R3c and is absent in the XRD data (Fig. <ref type="figure">2a</ref>). This suggests the possibility of long-range magnetic ordering which was further corroborated by the subsequent magnetization measurement.</p><p>The reflection at 4.56 &#197; in PND data disappears at high temperatures which is consistent with magnetic measurements (Fig. <ref type="figure">2c</ref> and Fig. <ref type="figure">3a</ref>). Preliminary magnetic structure analysis suggests a G-type antiferromagnetic ordering with magnetic moments predominantly aligned in the a-b plane (Fig. <ref type="figure">S4b</ref>, Supporting Information). The refined magnetic moment is 3.07 &#956; B and matches closely with the existing reports in BiFe 1-</p><p>x Ti x O 3 and Bi 1-x Sr x FeO 3 <ref type="bibr">[23,</ref><ref type="bibr">25]</ref>.</p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head n="3.3.">Magnetic properties</head><p>Magnetization data collected on BCFT15 in the temperature range of 2 to 400 K show that Zero-field cooled (ZFC) and Field cooled (FC) curves diverge from 400 K and remain down to 2 K (Fig. <ref type="figure">S5</ref>, Supporting Information). No magnetic anomalies were observed in this temperature range, therefore, excluding any spin-reorientation transition as observed in BiFeO 3 at 140 K and 200 K. Further magnetization isotherms collected at room temperature show a magnetic hysteresis loop. The presence of ZFC -FC divergence and magnetic hysteresis loop confirms weak ferromagnetism or canted antiferromagnetic behavior as commonly observed in rare-earth orthoferrites LnFeO 3 due to spin-canting. To determine the magnetic ordering temperature, ZFC and FC magnetization were measured in the oven option of the Physical property measurement system PPMS. As shown in Fig. <ref type="figure">3a</ref>, the sharp onset of FC magnetization and large divergence in ZFC -FC data confirm a magnetic ordering. This is also consistent with the nearly linear magnetic hysteresis loop at 600 K (Fig. <ref type="figure">3b</ref>). It may be noticed that the small hysteresis at 600 K and slight divergence in ZFC -FC data above T N may indicate a small amount of magnetic secondary phases which could not be identified using laboratory X-ray data. In particular, the presence of magnetic secondary phases in BiFeO 3 -related materials is a complex problem and depends on various other factors such as purity of starting materials, Bi-loss, phase homogeneity, etc <ref type="bibr">[28,</ref><ref type="bibr">31]</ref>. The onset of the magnetic ordering as determined from the derivative of FC data is T N = 557 K. The remanent magnetization (M r ) at 300 K is estimated from the M-H isotherm to be 0.01 &#956; B /f.u. The appearance of weak ferromagnetism in BCFT15 can be understood as follows. Unlike in rare earth orthoferrites, the net magnetization caused by antisymmetric Dzyaloshinsky-Moriya interaction is zero due to the incommensurately modulated spin structure below T N = 643 K <ref type="bibr">[46,</ref><ref type="bibr">47]</ref>. Substitution of nonmagnetic Ti 4+ in the Fe 3+ site and Ca 2+ in the Bi 3+ site perturbs the spatial spin structure and this, in turn, induces canted antiferromagnetic behavior as observed in orthoferrites and BiFeO 3 -CaTiO 3 <ref type="bibr">[25,</ref><ref type="bibr">44,</ref><ref type="bibr">48]</ref>.</p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head n="3.4.">Dielectric, and ferroelectric properties</head><p>The room temperature dielectric constant in BCFT15 varies from 86 to 77 in the frequency range of 100 Hz to 1 MHz. Interestingly the dielectric loss is low and ranges from 0.01 to 0.03 in the same frequency range (Fig. <ref type="figure">4a</ref>). It should be noted that the processing of BiFeO 3 and related ceramic oxides is challenging, and high dielectric loss can result in artifacts in ferroelectric measurements. The loss data presented here is similar to the reported values in BiFeO 3 -CaTiO 3 system <ref type="bibr">[44]</ref>. The low loss in these oxides facilitated measurements up to 180 kV/cm during ferroelectric polarization versus electric field (P(E)) loop measurements. As the external field increases, the polarization data evolves in a nonlinear way (Fig. <ref type="figure">4c</ref>) indicating domain wall motion <ref type="bibr">[27,</ref><ref type="bibr">49]</ref>. It should be cautioned that the loops presented here do not demonstrate ferroelectricity and may require the application of a higher electric field for polarization switching.</p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head n="3.5.">Complex impedance study</head><p>To understand the origin of the dielectric behavior, the complex impedance spectroscopy (CIS) technique was employed. Fig. <ref type="figure">5a</ref>, <ref type="figure">b</ref> and Fig. <ref type="figure">5d</ref>, e shows the complex impedance spectra (Nyquist plot) at selected temperatures for BCFT15 and BSFT15 respectively. The impedance plots at lower temperatures can be explained in terms of a single contribution arising from grains. The data has been modeled using a parallel circuit consisting of resistance (R) and a constant phase element CPE (Y CPE = 1 ZCPE = A 0 (j&#969;) n ) where A 0 and n are constants for a given temperature (0 &#8804; n &#8804; 1). The equivalent capacitance (C = R</p><p>) is of the order of 10 -11 F suggesting a contribution from the grains <ref type="bibr">[50]</ref>. The activation energy (E a ) is obtained from the grain conductivity (&#963; dc ) vs 10 3 /T plot using Arrhenius equation (&#963; dc = &#963; 0 e -Ea k B T ) <ref type="bibr">[51]</ref>. The activation energy obtained from the linear fit is 1.15(9) eV and 1.16 <ref type="bibr">(4)</ref> eV respectively for BCFT15 and BSFT15 compositions (Fig. <ref type="figure">5c</ref>, <ref type="figure">f</ref>). The compositions show predominantly grain contribution between 500 K and 623 K whereas above 650 K an additional arc appears in the impedance plots as shown by blue arrows (Fig. <ref type="figure">5b</ref>, <ref type="figure">e</ref>). The equivalent capacitance is found to be of the order of 10 -6 F indicating electrode contribution <ref type="bibr">[24,</ref><ref type="bibr">50]</ref>.</p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head n="4.">Conclusions</head><p>We explored BiFeO 3 -Bi 2/3 TiO 3 -ATiO 3 where (A 2+ = Ca 2+ , Sr 2+ , Ba 2+ ) ternary phase diagram and achieved perovskite phases with high-bismuth content at the A-site. Preliminary Rietveld measurements suggest a polar rhombohedral structure (Space group R3c) akin to the parent BiFeO 3 . These compositions show a low dielectric loss, and the electrical response is dominated by grain contribution. PND and DC magnetic measurements confirm long-range magnetic ordering below 557 K. At room temperature, these compositions are both polar and weak ferromagnetic. The strategy would be helpful to design new roomtemperature polar magnetic materials.</p></div></body>