			<titleStmt><title level='a'>Nanofibrous mat-enabled soil water absorption for continuous soil nitrate sensing</title></titleStmt>
			<publicationStmt>
				<publisher>Elsevier</publisher>
				<date>07/01/2025</date>
			</publicationStmt>
			<sourceDesc>
				<bibl> 
					<idno type="par_id">10584422</idno>
					<idno type="doi">10.1016/j.compag.2025.110319</idno>
					<title level='j'>Computers and Electronics in Agriculture</title>
<idno>0168-1699</idno>
<biblScope unit="volume">234</biblScope>
<biblScope unit="issue">C</biblScope>					

					<author>Vignesh Kumar Haridass</author><author>Michael J Castellano</author><author>Liang Dong</author>
				</bibl>
			</sourceDesc>
		</fileDesc>
		<profileDesc>
			<abstract><ab><![CDATA[Continuous monitoring of soil nitrate levels is essential for effective soil nutrient management. However, limited soil pore water at low soil water content levels hinders miniaturized soil sensor surfaces from efficiently interacting with nutrient ions. To address this, we introduce a nanofibrous mat designed to enhance nitrate detection by increasing connectivity between miniature sensors and the soil solution. Composed of polysulfone, polymethylmethacrylate, and polyvinyl alcohol, this mat is fabricated using electrospinning and electrospray methods to balance water absorbency, mechanical durability, and ease of manufacturing. When wrapped around  an ion-selective electrode-based nitrate sensor, the mat improves access to soil pore water, acts as a filter,  prevents direct sensor-soil particle contact, and reduces the impact of soil particle surface charges on sensor measurements. Continuous nitrate monitoring with both mat-wrapped and bare sensors was conducted in controlled and field environments. Linear regression analysis indicates that the mat-wrapped sensor has a  stronger correlation with conventional salt extract methods for measuring soil nitrate levels. T-tests confirm statistically significant differences between sensor measurements and the salt extraction method. Additionally, Bland-Altman analysis reveals that mat-wrapping reduces mean bias and narrows the limits of agreement, demonstrating improved agreement with the conventional method. Notably, the mat-wrapped sensor performs consistently across varying soil moisture conditions. These findings suggest that the water-absorbing mat improves the ability of the sensor to monitor nitrate continuously by accommodating varying soil moisture levels over time, making the mat-wrapped soil nitrate sensor a viable improvement for in-field measurements of soil solution chemistry.]]></ab></abstract>
		</profileDesc>
	</teiHeader>
	<text><body xmlns="http://www.tei-c.org/ns/1.0" xmlns:xsi="http://www.w3.org/2001/XMLSchema-instance" xmlns:xlink="http://www.w3.org/1999/xlink">
<div xmlns="http://www.tei-c.org/ns/1.0"><head n="1.">Introduction</head><p>Soil nitrogen (N) is essential for plant growth and external inputs of N fertilizer are required for crop production. However, determining the optimal amount of N fertilizer input is challenging because the soil naturally provides a large, but highly uncertain, amount of N in the form of nitrate (NO - 3) <ref type="bibr">(Bowles et al., 2018)</ref>. Greater certainty about how much nitrate the soil provides before and during crop growth would improve yields and environmental outcomes. One solution is to use inexpensive soil nitrate sensors to obtain real-time data on soil nitrate levels. Soil nitrate levels, measured with conventional methods, are well known to aid decision-making for agricultural management <ref type="bibr">(Ali et al., 2019;</ref><ref type="bibr">Baumbauer et al., 2022;</ref><ref type="bibr">Chen et al., 2024;</ref><ref type="bibr">Fan et al., 2022;</ref><ref type="bibr">Grell et al., 2021)</ref>. However, continuous soil nitrate sensors offer significant advantages over conventional methods because conventional methods are costly, time-consuming, and do not provide real-time information. Therefore, there is a growing demand for low-cost, accurate, continuous soil nitrate sensors to enhance agricultural management practices.</p><p>Several low-cost soil nitrate sensing methods have been developed, including electrochemical sensors <ref type="bibr">(Essousi et al., 2019;</ref><ref type="bibr">Sookhakian et al., 2021)</ref>, microfluidic-chip sensors <ref type="bibr">(Khanfar et al., 2017;</ref><ref type="bibr">Murphy et al., 2021)</ref>, and ion-selective electrodes (ISE) <ref type="bibr">(Ali et al., 2019;</ref><ref type="bibr">Chen et al., 2024;</ref><ref type="bibr">Fan et al., 2022;</ref><ref type="bibr">Zhu et al., 2021)</ref>. While many electrochemical sensors utilize ion-specific enzymes for molecular recognition, their long-term performance can be affected by enzyme stability <ref type="bibr">(Ahmad et al., 2017)</ref>. Microfluidic chips, which integrate electrophoretic separation mechanisms and electrochemical sensors, have been designed to measure multiple ions in soil water simultaneously but face challenges in extracting soil water for continuous measurement <ref type="bibr">(Kung et al., 2019;</ref><ref type="bibr">Xu et al., 2017)</ref>. ISE sensors have gained considerable attention due to their simple structure, rapid response, and compact size. Significant efforts have been made to address issues such as potential drift, interference from non-target species in the soil <ref type="bibr">(Chen et al., 2021;</ref><ref type="bibr">Shishkanova et al., 2011)</ref>, biofouling of ion-selective membranes (ISM) <ref type="bibr">(Szigeti et al., 2006)</ref>, inconsistency in sensor production, and instability of pseudo-reference electrodes <ref type="bibr">(Hu et al., 2016)</ref>. Essentially, ISE sensors operate on the principle of equilibrium concentration between the ISE surface and the surrounding solution, requiring both reference and working electrodes to be exposed to liquid solutions or wet environments <ref type="bibr">(Jackson and Nelson 2019;</ref><ref type="bibr">Zdrachek and Bakker 2018)</ref>. However, a notable challenge with deployment of ISM materials in soils is that they generally possess hydrophobic properties that repel aqueous solutions, hindering the movement of target ions into the membrane <ref type="bibr">(Chen et al., 2024;</ref><ref type="bibr">Fan et al., 2022)</ref>. This issue is exacerbated when soil moisture levels are low. The mixed solid-gas-solution composition of soil leads to inconsistent interaction between the sensor and soil solution, leading to inaccurate and inconsistent measurements over time.</p><p>To solve this issue, several methods have been suggested to draw soil pore water, thereby bringing mobile ions into contact with the sensor surface <ref type="bibr">(Bieg et al., 2017;</ref><ref type="bibr">Wang et al., 2022)</ref>. For example, surface modification techniques using self-assembled functional groups like -COOH, -OH, and -NH2 can create a hydrophilic sensor surface. Similarly, other treatments, such as plasma treatment with ultraviolet and ozone, allow for enhancing wettability by increasing the presence of -OH groups. Another approach involves depositing metal oxide nanoparticles onto the sensor surface. Despite these efforts, nitrate sensors still face significant instability and unreliability when soil water content decreases <ref type="bibr">(Chen et al., 2024)</ref>. A recent, promising method involves coating the sensor surface with a thin hydrogel layer and a hydrophilic polyvinylidene fluoride (PVDF) layer to facilitate ion transport from the soil to the sensor surface <ref type="bibr">(Chen et al., 2024;</ref><ref type="bibr">Fan et al., 2022)</ref>. However, a drawback of using hydrogel is mechanical weakness, which compromises the durability and structural integrity of the sensor <ref type="bibr">(Hu et al., 2023;</ref><ref type="bibr">Sun et al., 2020)</ref>. Additionally, the ability of hydrophilic PVDF to promote long-term nitrate measurements under field conditions remains unknown <ref type="bibr">(Chen et al., 2024)</ref>.</p><p>This paper presents a nanofibrous mat designed to enhance soil water absorption, improving the performance of an ISE-based nitrate sensor. By drawing soil pore water toward the sensor surface, the mat increases surface wetness, ensuring connectivity between the sensor surface and the soil water for continuous nitrate detection (Fig. <ref type="figure">1</ref>). Its high hydrophilicity and efficient water absorption overcome a common challenge faced by many miniaturized soil nitrate sensors, which often perform poorly under low soil moisture conditions due to limited interaction with nutrient ions in soil pore water. The mat ensures consistent ion detection across varying soil moisture levels. Furthermore, its enhanced mechanical strength prevents the sensor from potential damage caused by direct contact with soil particles. The porous structure of the mat also acts as a filter, allowing soil water to reach the sensor while reducing the impact of surface charges from soil particles on the sensor output. This </p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head>&#215;</head><p>nanofibrous mat enables more reliable and robust soil nitrate sensing across diverse soil moisture conditions.</p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head n="2.">Experimental</head></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head n="2.1.">Nanofibrous mat design</head><p>The nanofibrous mat was composed of polysulfone (PSF), polymethylmethacrylate (PMMA), and polyvinyl alcohol (PVA) and was formed through a combination of electrospinning and electrospray <ref type="bibr">(Huang et al., 2022)</ref> techniques (Fig. <ref type="figure">1c</ref>). Initially, PSF-PMMA nanofibers were produced via electrospinning, and then PVA was applied to the PSF-PMMA nanofiber surface through electrospray, followed by using a cross-linking method to stabilize the PVA on the surface of the PSF-PMMA nanofibers. The design of this mat balanced water absorbency, mechanical durability, and ease of manufacturing. Specifically, PSF provided high mechanical strength, fouling resistance, and thermal and chemical stability <ref type="bibr">(Chee et al., 2022)</ref>. However, due to poor electrospinnability, PSF nanofibers tended to agglomerate <ref type="bibr">(Obaid et al., 2015)</ref>. This issue was mitigated by incorporating PMMA, which improved the electrospinnability of the PSF-PMMA nanofibers <ref type="bibr">(Wu et al., 2022;</ref><ref type="bibr">Xu et al., 2018)</ref>. The hydrophobic nature of PSF-PMMA nanofibers, however, impeded soil water absorption, a crucial drawback addressed by coating the nanofibers with hydrophilic PVA <ref type="bibr">(Park et al., 2018)</ref>. Directly blending PVA with the PSF-PMMA precursor solution for electrospinning would result in phase separation due to the incompatibility between the hydrophobic characteristics of PSF-PMMA and the hydrophilic characteristics of PVA <ref type="bibr">(Li et al., 2020)</ref>.Therefore, PVA was electrosprayed onto the PSF-PMMA nanofibers. To ensure the stability of PVA in soil water, the PVA-coated PSF-PMMA (or PVA/PSF-PMMA) nanofibers were treated with a malic acid solution. This treatment facilitated cross-linking between the carboxylic groups of malic acid and the hydroxyl groups of PVA <ref type="bibr">(Vald&#233;s et al., 2021)</ref> thus stabilizing the PVA/PSF-PMMA nanofibrous mat in water.</p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head n="2.2.">ISE sensor manufacturing</head><p>The manufacturing method of the ISE nitrate sensor used in this study (Fig. <ref type="figure">1a</ref>) is detailed in our previous work <ref type="bibr">(Ali et al., 2019)</ref>. Briefly, the sensor comprised a working electrode (WE; 2.5 mm diameter) and a reference electrode (RE; 2.5 mm diameter) on a printed circuit board (PCB). The conducting base electrodes and wires of the sensor were made of copper on the PCB. The WE consisted of a 10 nm-thick titanium (Ti) layer, a 250 nm-thick gold (Au) layer, a nanocomposite of poly(3octyl-thiophene) (POT), and molybdenum disulfide (MoS2) serving as an ion-to-electron transducing layer, and an ISM for nitrate selection <ref type="bibr">(Ali et al., 2019)</ref>. To prepare the POT-MoS2 nanocomposite, 2.6 mg of POT was dissolved in 1 mL of tetrahydrofuran (THF) solvent. Then, 10.4 mg of MoS2 was added. The mixture was sonicated for 4 h to achieve a uniform dispersion. The NO - 3 -ISM was prepared by mixing the following components, including 1.50 wt% of tridodecylmethylammonium nitrate, 5.75 wt% of polyvinyl chloride, 16.25 wt% of 2-nitrophenyl octyl ether, 0.25 wt% of methyltriphenylphosphonium bromide, 1.93 wt% of nitrocellulose (moistened with 2-propanol), and 74.3 wt% of THF. The mixture was stirred at 1500 rpm and 30 &#8451; for 12 h to obtain a homogeneous solution <ref type="bibr">(Ali et al., 2019)</ref>. The RE consisted of a 500 nm-thick silver (Ag) layer, a 500 &#956;m-thick Ag/AgCl paste layer, and an 80 nmthick protonated Nafion layer to minimize chloride ion leaching to the surrounding environment. Waterproof epoxy covered the device, exposing the WE and RE to the soil. Before use, the sensor was preconditioned by immersion in a 2500 ppm NO - 3 solution for 24 h (Zhu et al., 2021).</p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head n="2.3.">Formation of PVA/PSF-PMMA nanofibers</head><p>Initially, a mixture solution of PSF-PMMA was prepared by dissolving 1.2 g PSF pellets (Sigma-Aldrich; MO, USA) and 0.3 g PMMA powder (Sigma-Aldrich; MO, USA) in 8.5 mL N, N-dimethylformamide (DMF; Sigma-Aldrich; MO, USA). This mixture was stirred at 1100 rpm and 60 &#8226; C for 12 h to obtain homogeneous dissolution. Subsequently, for the electrospinning of PSF-PMMA nanofibers, a 27 kV DC voltage (Gamma High Voltage Research, FL, USA) was applied between a metal spinneret and a fiber collector (Fig. <ref type="figure">1c</ref>). The spinneret consisted of a blunt-end metal needle with an inner diameter of 0.84 mm and an outer diameter of 1.27 mm (gage size: 18G; Nordson EFD, OH, USA). The fiber collector was a stainless flat plate (15.3 12.7 cm) covered with 1 mm thick aluminum foil (Reynolds Wrap, IL, USA). The spinneret-tocollector distance was set at 10 cm. The polymer mixture solution of PSF-PMMA was loaded into a 10 mL syringe driven by a syringe pump (catalog #14-831-200; Fisher Scientific, NH, USA) at a feed rate of 1.5 mL/h. During electrospinning, the electric field stretched the polymer solution into elongated fibers, which were then deposited onto the collector as PSF-PMMA nanofibers.</p><p>To electrospray PVA on the PSF-PMMA nanofibers, a PVA solution was prepared by dissolving 1.2 g PVA (Sigma-Aldrich, MO, USA) in 8.8 mL dimethylsulfoxide (DMSO; Sigma-Aldrich; MO, USA) and stirring the mixture at 1100 rpm at 70 &#8226; C for 2 h to achieve a homogeneous solution. This solution was then electrosprayed onto the PSF-PMMA nanofibers using the same setup and conditions as described for the electrospinning process. However, unlike the nanofiber formation observed with electrospinning, the PVA solution formed droplets (Fig. <ref type="figure">1c</ref>) due to the higher boiling point of DMSO (189 &#8226; C), which limited solvent evaporation during the process. To ensure complete evaporation of the DMSO from the PVA droplets, the PVA-coated PSF-PMMA mat was placed in a vacuum-drying oven at 90 &#8226; C for 8 h. After that, the dried mat was wrapped around the ISE sensor. The sensor with the mat was immersed in a 1 % crosslinker solution of malic acid (MA; Sigma-Aldrich; MO, USA) for 12 h (Fig. <ref type="figure">1c</ref>). Finally, the sensor was rinsed with deionized water to remove residual solvents.</p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head n="2.4.">Fiber characterization</head><p>Surface morphology of the pristine PSF, PSF-PMMA, and PVA/PSF-PMMA nanofibers were examined using a scanning electron microscope (FEI Quanta-FEG 250, OR, USA). Attenuated total reflectance-Fourier transform infrared (ATR-FTIR) spectroscopy (Bruker Tensor 37, MA, USA) was used to examine the surface functionalities of these nanofibers. Additionally, the hydrophilicity of these nanofibers was evaluated by measuring their water contact angles on a homemade goniometer.</p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head n="2.5.">Sensor characterization using treated soils</head><p>Sensor characterizations were conducted using soil collected from the Iowa State University Agronomy and Agricultural Engineering Research Farm. The soils were washed, air-dried, and sterilized in a muffle furnace at 400 &#8451; to reduce microbial activity <ref type="bibr">(Zhu et al., 2021)</ref>. The sterilized soil was then adjusted to a bulk density of 1.25 g cm -3 and prepared with three gravimetric soil water contents (0.2, 0.3, and 0.4 g/ g) and five soil solution NO - 3 concentrations (10, 25, 50, 75, and 100 mg/L). These gravimetric soil water contents and NO - 3 concentrations were chosen because they encompass the typical ranges observed during the growing season in the rainfed Corn Belt maize fields <ref type="bibr">(Zhu et al., 2021)</ref>. Each sensor was installed in the center of each cup for measurements.</p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head n="2.6.">Field study</head><p>Field studies were conducted to assess the performance of matwrapped and bare ISE sensors. These devices were deployed at two adjacent locations (~40 cm apart) at the Iowa State University Agronomy and Agricultural Engineering Research Farm. Both types of sensors were placed approximately 25 cm beneath the surface soil at each location. Sensor readings (measured in mV) were recorded at 20minute intervals from September 17 to October 11, 2023. Sensors were considered functional when the difference between the pre-and post-deployment calibration curves was less than 20 % <ref type="bibr">(Zhu et al., 2021)</ref>.</p><p>To obtain ground-truth nitrate levels in the soil, samples were collected from locations close to the installed sensors and analyzed using the salt extract method <ref type="bibr">(Zhu et al., 2021)</ref>. These samples were mixed with 2 M KCl solution (1:5 soil-to-solution ratio) and shaken reciprocally for 1 h at 180 rpm. The soil slurry was then filtered using Whatman #1 filter paper, and the filtrates were refrigerated until analysis. The NO - 3 concentrations (mg/L) of the filtrates were measured with colorimetry in microplates using the Griess-Ilosvay reaction with VCl3 as a reagent <ref type="bibr">(Zhu et al., 2021)</ref>.</p><p>To convert the NO - 3 concentration in the filtrate (mg/L of) to mg/kg of dry soil, the gravimetric soil water content was first calculated using the equation: Gravimetric soil water content (g/g) = [Weight of wet soil (g) -Weight of oven-dried soil (g)] / Weight of oven-dried soil (g)] <ref type="bibr">(Hack, 1984)</ref> and then the conversion was completed using the equation (Zhu et al., 2021): NO - 3 (mg/L) soil solution &#215; gravimetric soil water content (g/g) = NO - 3 (mg/kg) of dry soil.</p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head n="3.">Results and discussion</head></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head n="3.1.">Material characterization</head><p>Fig. <ref type="figure">2a</ref> shows the surface morphology of PSF nanofibers, which were aggregated during electrospinning due to intermolecular hydrogen bonding between PSF molecules. For the PSF-PMMA nanofibers, the microstructure of the PSF matrix transforms because PMMA was dispersed throughout the PSF matrix, reducing the opportunities for intermolecular hydrogen bonding between PSF molecules. This disruption minimized the tendency of PSF molecules to aggregate during electrospinning (Fig. <ref type="figure">2b</ref>). Additionally, electrosprayed PVA beads were used to modify the PSF-PMMA (Fig. <ref type="figure">2c</ref>). The formation of the PVA beads instead of fibers was associated with the slow evaporation of the DMSO solvent. DMSO has a high boiling point, making it difficult to evaporate completely during the electrospraying process. When the solvent evaporated slowly, the polymer solution remained in a more liquid state for a longer period, preventing the formation of continuous fibers. Instead, the solution tended to form droplets, which solidified into beads as the solvent gradually evaporated.</p><p>The water contact angle measurement (Fig. <ref type="figure">2d-2f</ref>) showed that the PSF and PSF-PMMA nanofibers exhibited a similar contact angle of ~84 &#8226; . However, the surface modification with sprayed PVA significantly reduced the contact angles to nearly zero, indicating enhanced = n hydrophilicity. This improvement was attributed to the presence of water-soluble -OH groups in PVA. Additionally, to demonstrate the high mechanical strength, the mat was clamped on both sides using a paper clip and tested by lifting a 192 g iron base of a soldering welding stand.</p><p>surface interactions between the mats and nitrate ions. The Langmuir model was applied to study the monolayer sorption of nitrate ions on the mat surface. The linearized Langmuir model is represented by Equation (1) <ref type="bibr">(Santos et al., 2020;</ref><ref type="bibr">Song et al., 2016)</ref>: The mat maintained its integrity during the test (Fig. <ref type="figure">2g</ref>). Further, the Ce 1 Ce mat was capable of filtering water from a soil-mixed water sample. In this experiment, a mixture of soil and water was gradually loaded onto the mat affixed to the opening of a vial. Most soil particles were filtered out and remained on the mat, while the water infiltrated into the vial (Fig. <ref type="figure">2h</ref>).</p><p>Fig. <ref type="figure">3</ref> shows the FTIR spectra of the pristine PSF, PSF-PMMA, and PVA/PSF-PMMA nanofibers. The peaks at 633 and 696 cm -1 indicated the stretching vibrations of C-O and C-S bonds, respectively. Additionally, the peaks at 1148, 1237, and 1323 cm -1 were associated with the sulfonyl group (O=S=O), while the peak at 1295 cm -1 indicated the presence of the aromatic ether group (C-O-C) (Sadare and Daramola 2021). The peaks observed in the 832-873 cm -1 range were associated with the stretching vibrations of C C bonds within the aromatic ring structure (Fig. <ref type="figure">3a</ref>). Also, the peak in the 2869-2998 cm -1 range was attributed to the stretching of C-H bonds in alkane moieties (Fig. <ref type="figure">3b</ref>). Furthermore, compared to the pristine PSF, a new peak appeared at 1729 cm -1 for PSF-PMMA and PVA/PSF-PMMA, indicating the stretching vibration of -COOCH3 in PMMA (Fig. <ref type="figure">3a</ref>). The broad band</p><p>where Ce (mg/L) is the equilibrium concentration of nitrate, qe (mg/g) is the amount of nitrate adsorbed per unit mass of the mat, Qmax (mg/g) is the maximum adsorption capacity, and KL (L/mg) is the Langmuir constant related to the adsorption binding energy. From the linear plot of Ce/qe versus Ce, the calculated Qmax was 7.17 mg/g, and the Langmuir constant KL was determined to be 0.063 L/mg, with a correlation coefficient (r 2 ) of 0.93. These results indicated that nitrate adsorption primarily occurs as a monolayer on a homogeneous surface. The Freundlich equation, another equilibrium isotherm model that describes adsorption onto heterogeneous surfaces, is expressed by Equation ( <ref type="formula">2</ref>) <ref type="bibr">(Santos et al., 2020;</ref><ref type="bibr">Song et al., 2016)</ref>:</p><p>where KF mg/g(L/mg) 1/n is the Freundlich constant, indicative of observed at 3406 cm -1 in the PVA/PSF-PMMA spectra (Fig. <ref type="figure">3b</ref>) was due to the stretching vibration of O-H in PVA, confirming that PVA was successfully coated on the PSF-PMMA nanofibers by the electrospray process.</p><p>The water absorption study for the PVA/PSF-PMMA nanofibrous mat was conducted to assess the capacity of the mat to absorb water. Initially, the mat was weighed in its dry state and then immersed in 20 mL of deionized water for 24 h at room temperature. After soaking, the mat was reweighed, and the weight difference was used to calculate the amount of water absorbed <ref type="bibr">(Sim et al., 2023)</ref>. A 0.1 g dry mat absorbed approximately 0.1 g of water, confirming its considerable water absorption capability.</p><p>To evaluate the ion sorption capacity of the mat, five identical 0.1 g dry mats were individually immersed in 20 mL nitrate solutions with concentrations of 10, 25, 50, 75, and 100 ppm, respectively. The mats were left in immersion for 24 h at room temperature to ensure sufficient interaction with nitrate ions <ref type="bibr">(Mohammad and Atassi 2020)</ref>. After that, the remaining nitrate concentrations in the solutions were measured using a spectrophotometer.</p><p>The equilibrium adsorption isotherms for nitrate adsorption onto the nanofibrous mats were analyzed using the Langmuir and Freundlich isotherm models <ref type="bibr">(Santos et al., 2020;</ref><ref type="bibr">Song et al., 2016)</ref>. Fig. <ref type="figure">4</ref> illustrates the adsorption isotherms, demonstrating the adsorption capacity and adsorption capacity, and 1/n is a Freundlich intensity parameter that represents the adsorption strength. The linear plot of log qe versus log Ce provided a KF value of 0.79 mg/g(L/mg) 1/n and an n value of 1.9, with a high r 2 value of 0.99. The n value greater than 1 suggests favorable adsorption, while the high r 2 value indicated an excellent fit of the Freundlich model to the experimental data.</p><p>The theoretical parameters for both isotherm models are summarized in Table <ref type="table">1</ref>. The dual fitting of the data using the Langmuir and Freundlich models demonstrated the ability of the mat to support both homogeneous and heterogeneous adsorption mechanisms. These results suggested that the primary role of the mat in sensing applications was to facilitate nitrate ion transport to the sensor interface without significantly sequestering or obstructing the ions.</p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head n="3.2.">Sensor calibration and characterization</head><p>Both the nitrate sensor wrapped with the PVA/PSF-PMMA mat and its bare counterpart were characterized in the laboratory using pretreated soil samples with varying nitrate concentrations ranging from 10 to 100 mg/kg at a constant soil water content of 0.4 g/g (see Section 2.5 for sample preparation details). Following each measurement, the sensors were rinsed with DI water to remove residual soil and dried with nitrogen before testing the next sample. This procedure was repeated for ----Fig. 4. (a) Langmuir isotherm for monolayer nitrate adsorption on the surface of the PVA/PSF-PMMA nanofibrous mat, showing the relationship between Ce/qe and Ce. (b) Freundlich isotherm for nitrate adsorption on the surface of the PVA/PSF-PMMA nanofibrous mat, showing the relationship between log (qe) and log (Ce).</p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head>Table 1</head><p>Isotherm parameters for nitrate ion adsorption onto the PVA/PSF-PMMA mat.</p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head>Isotherm model Parameter Value</head><p>Langmuir Qmax (mg/g) 7.17 KL (L/mg) 0.063 r 2 0.93 by 2 % with 50 mg/kg NO - 3 and 50 mg/kg PO 3 4 -. Notably, the response increased by 16 % with 50 mg/kg NO - 3 and 50 mg/kg NO - 2 , likely due to the molecular similarity between NO - 3 and NO - 2 . To evaluate the recyclability of the mat-wrapped sensor, tests were conducted using six soil samples, each containing 25 mg/kg of nitrate at a constant gravimetric soil water content of 0.4 g/g (see Section 2.5 for sample preparation details). After each measurement, the sensor was</p><p>Freundlich n KF (mg/g) (L/mg) 1/n 1.9 0.79 thoroughly washed with DI water to remove residual soil and nitrate r 2 0.99 five different soil nitrate concentrations. The output voltage signals of both types of sensors significantly changed with increasing concentrations of NO - 3 (Fig. <ref type="figure">5a</ref>, <ref type="figure">5b</ref>). Their calibration plots exhibited linear relationships between the output voltage and the logarithmic concentration of NO - 3 (Fig. <ref type="figure">5c</ref>, <ref type="figure">5d</ref>). The sensitivity and the correlation coefficient obtained from the calibration plots were found to be 54.93 mV/dec and 0.99, respectively, for the mat-wrapped sensor and 54.24 mV/dec and 0.99 for the bare sensor. Therefore, the PVA/PSF-PMMA nanofibrous mat did not compromise the sensitivity of the sensor to detect nitrate ions. It should be noted that the potential difference between the mat-wrapped sensor and its bare counterpart for the same nitrate concentration might be attributed to the inherent variability in soil media which the ISM of each sensor was exposed.</p><p>The reproducibility of the mat-wrapped sensor was evaluated by measuring the NO - 3 concentration (25 mg/kg) in the pretreated soil (see Section 2.5 for sample preparation details). using five identical sensors produced from the same batch. These sensors provided similar calibration curves, with their sensitivities between 52.31 and 56.62 mV/dec (Fig. <ref type="figure">5e</ref>). The histogram in the inset of Fig. <ref type="figure">5e</ref> shows the response concentrations of these sensors using their respective calibrations. The relative standard deviation of the measured concentrations across these sensors was ~3 %, indicating considerable reproducibility of the matwrapped sensors.</p><p>To evaluate the selectivity of the mat-wrapped sensor, various ions were added to soil samples, including 50 mg/kg NO - 3 alone, and mixtures of 50 mg/kg NO - 3 with 50 mg/kg of interference ion (Cl -, HCO - 3 , SO 2 4 -, PO 3 4 -, or NO - 2 ) (Fig. <ref type="figure">5f</ref>). A blank soil sample without any added ions was also tested by the sensor, which indicated negligible (i.e., irrelevant for agricultural decision making) nitrate concentrations of ~2 mg/kg. When 50 mg/kg of NO - 3 was added to this blank soil sample, the sensor response increased to ~51 mg/kg NO - 3 . The sensor response varied when interference ions were present: it decreased by 8 % with 50 mg/kg NO - 3 and 50 mg/kg Cl -, by 4 % with 50 mg/kg NO - 3 and 50 mg/ kg HCO - 3 , by 2 % with 50 mg/kg NO - 3 and 50 mg/kg SO 2 4 -, and increased before being reused with the next soil sample. This process was repeated for six cycles, during which the sensor response was monitored to assess its reusability. The histogram in Fig. <ref type="figure">5g</ref> illustrates the sensor readout of nitrate concentrations across these cycles. The relative standard deviation of the measured concentrations was ~8 %, demonstrating the good recyclability and consistent performance of the mat-wrapped sensor over multiple uses.</p><p>Both mat-wrapped and bare sensors were exposed to a 50 mg/kg NO - 3 concentration at varying soil water contents (0.2-0.4 g/g) in a controlled environment. Each soil container, with a specified soil water content, housed both a mat-wrapped and a bare sensor for 17 days. The lower panel of Fig. <ref type="figure">6a</ref> shows that at 0.2 g/g water content, the bare sensor exhibited an unstable response during the measurement; this instability was likely due to the limited ability of the sensor to draw soil water to its surface and the influence of charged soil particles on its voltage output. Interestingly, the bare sensor took 4-5 days to reach a relatively stable response at 0.3 g/g of soil water content (the middle panel of Fig. <ref type="figure">6a</ref>) and only 2-3 days at 0.4 g/g of soil water content (the upper panel of Fig. <ref type="figure">6a</ref>). These results indicated that higher soil water contents are favorable for the bare sensor to conduct soil nitrate measurements.</p><p>In contrast, the mat-wrapped sensor in soil with 0.2 g/g water content exhibited a more consistent response after 2-3 days compared to the bare sensor at the same water content level. At 0.3 g/g water content, the mat-wrapped sensor took 1-2 days to reach a relatively stable voltage output, while at 0.4 g/g water content, the sensor achieved signal stabilization within one day (Fig. <ref type="figure">6b</ref>). These results suggested that the PVA/PSF-PMMA mat improved the signal stability of the nitrate sensor under varying gravimetric soil water contents. Additionally, the time required for the mat-wrapped sensor to reach a stable response depended on the soil water content level, with higher soil water content levels allowing the sensor to stabilize more quickly by drawing water to its surface. These soil water contents represent the full range of water contents typically observed during early season maize growth when nitrogen fertilizer management decisions are made.  </p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head n="3.3.">Field sensing of soil nitrate</head><p>The field measurement capabilities of the mat-wrapped and bare soil nitrate sensors were assessed. Details of sensor installation, soil sampling, preparation, and salt extract measurement are provided in Section 2.6. Fig. <ref type="figure">7a</ref> shows that throughout the 24-day period, the mat-wrapped and bare sensors exhibited similar trends in soil nitrate changes over time. However, the wrapped sensor provided more detailed variations in soil nitrate concentrations than the bare sensor. For example, the wrapped sensor even revealed smaller but clear diurnal changes in soil nitrate concentrations over several days; however, such changes were barely by the bare sensor.</p><p>To evaluate the accuracy and reliability of the mat-wrapped and bare sensors compared to the salt extract method, linear regression, paired sample t-test, and Bland-Altman analyses <ref type="bibr">(Zhu et al., 2021)</ref> were performed. Linear regression was used to describe the relationship between sensor outputs (both mat-wrapped and bare) and the salt extract measurements (Fig. <ref type="figure">7b</ref>). The coefficient of determination (r 2 ) quantified the variance in the dependent variable (sensor output on the y-axis) explained by the independent variable (salt-extract data on the x-axis). The sensor data represented mean daily soil NO - 3 concentration on the sampling days: 9/20, 9/24, 9/28, 10/2, 10/6, and 10/9. The regression line for the mat-wrapped sensor was characterized by the equation y 0.633x 4.380 with an r 2 value of 0.944, indicating a strong correlation between the mat-wrapped sensor measurements and the salt extract method. The slope of 0.633 indicated that this sensor tended to underreport nitrate levels as compared to the conventional method. In contrast, the bare sensor data followed the equation y 0.735x-5.923 with an r 2 value of 0.821. While the r 2 value of the bare sensor indicated a reasonable correlation, it was lower than that of the mat-wrapped sensor. The 1:1 line in Fig. <ref type="figure">7b</ref> represented the ideal match between the sensor and salt extract measurements, but the actual slopes of both regression lines were below 1. This discrepancy arose from the different approaches used to assess soil NO - 3 concentration in different nitrogen pools. The salt extract method estimated the bioavailable nitrogen pool (including both inorganic and organic forms), while the sensors measured mobile nitrate ions in the soil pore water.</p><p>The paired sample t-tests revealed statistically significant differences between both sensor measurements and the salt extract method (p &lt; 0.001) (Fig. <ref type="figure">7b</ref>). The t-statistics, which represented the difference between sample means divided by the standard error of the difference, provided insight into the magnitude of the differences. A higher t-statistic reflected a larger discrepancy, while a lower value suggested closer agreement. Notably, the mat-wrapped sensor exhibited a lower t-statistic (t 6.92) compared to the bare sensor (t 12.64), indicating closer alignment with the salt extract method. The confidence interval (CI) complemented the t-test by providing a range where the true parameter (e.g., mean difference) is estimated to lie at a given confidence level (e.g., 95 %). A narrower CI indicates greater precision in the estimate. The mat-wrapped sensor exhibited a narrower CI (4.9 to 9.47 mg/kg) compared to the bare sensor (11.83 to 16.81 mg/kg), indicating reduced variability and improved measurement consistency. The CI was --------+ --</p><p>calculated from the sample mean, standard error, and a t-value corresponding to the desired confidence level and degrees of freedom. Moreover, the Bland-Altman analysis assessed the agreement between the salt extract and sensor (both wrapped and unwrapped) measurement data from Fig. <ref type="figure">7b</ref> against the mean of these two measurements. The Bland-Altman plot (Fig. <ref type="figure">7c</ref>) showed that the mean percentage difference between the bare sensor and the salt extract method was 62.56 %, indicating a substantial underestimation of nitrate levels by the bare sensor compared to the conventional method. The limits of agreement were calculated at 19.28 % (upper limit, 1.96 SD; SD means standard deviation) and 105.84 % (lower limit, 1.96 SD). The scatter of data points around the mean highlighted a consistent negative bias, with most points falling below the mean percentage difference. In contrast, the Bland-Altman plot for the mat-wrapped sensor (Fig. <ref type="figure">7d</ref>) displayed a mean percentage difference of 24.19 %, indicating a closer approximation to the conventional method compared to the bare sensor. The limits of agreement were narrower, with the upper limit at 7.11 % and the lower limit at 41.27 %. The data points for the mat-wrapped sensor were more tightly clustered around the mean, suggesting higher consistency and less variability in the measurements. The comparative analysis of the mat-wrapped and bare sensors revealed that the former outperformed the latter in terms of measurement reliability and consistency.</p><p>The uncertainty of the sensor measurement was analyzed across varying soil moisture levels. Fig. <ref type="figure">7e</ref> illustrates the percentage difference between the sensor and the salt extract method across various gravimetric soil water contents. For the mat-wrapped sensor, the percentage differences were relatively stable across a range of soil water contents from 0.15 to 0.40 g/g. This sensor consistently showed a percentage difference of around 20 %, indicating a relatively constant underestimation of nitrate levels compared to the conventional method. This stability suggested that the mat-wrapped sensor was less affected by varying soil moisture levels, providing reliable measurements under different soil moisture conditions. In contrast, the bare sensor exhibited a wider range of percentage differences, ranging from 120 % to 40 %. The data points for the bare sensor showed significant variability, particularly at lower soil water contents (0.15 to 0.25 g/g), where the percentage differences were more pronounced and erratic. This indicated that the accuracy of the bare sensor was highly influenced by soil moisture levels, especially in drier soil conditions.</p><p>Potential sources of error and uncertainty in sensor measurements include soil water content levels, interference from non-target ions, material degradation, surface charges on soil particles, and environmental impacts. Low soil water content can hinder ion mobility, reducing the efficiency of ion transport to the sensor surface. For instance, bare sensors exhibited unstable signal outputs under low soil water conditions (Fig. <ref type="figure">6a</ref>). Additionally, charged soil particles may induce voltage fluctuations, contributing to measurement inconsistencies. Interference from non-target ions, such as Cl -, K + , and PO 3 4 -, is another significant source of uncertainty, as shown in the selectivity tests (Fig. <ref type="figure">5f</ref>). While the mat-wrapped sensor mitigates some of these issues by promoting stable interaction with the soil solution, challenges remain due to factors such as material durability and interference ions.</p><p>A variety of low-cost nitrate sensing technologies have been reported, utilizing different detection mechanisms and materials, with varying levels of success in laboratory and field environments (Table <ref type="table">2</ref>). While many sensors performed well in controlled laboratory conditions, their application in field settings remains limited, particularly for soil nitrate monitoring. The ISE-based sensor presented in this study, enhanced with a PVA/PSF-PMMA nanofibrous mat, demonstrated effective soil nitrate monitoring across varying soil water content levels under both laboratory and field conditions over extended periods. Several other ISE sensors have also incorporated water-absorbing materials, such as PVDF and hydrogel, to improve interaction with soil; however, their testing was limited to laboratory settings. For example, hydrogel-coated ISE sensors showed stable performance for 14 days in lab conditions <ref type="bibr">(Fan et al., 2022)</ref>, and the PVDF-coated ISE sensors demonstrated reliable operation in laboratory soil tests <ref type="bibr">(Chen et al., 2024)</ref>. But, their suitability for field applications has yet to be evaluated. Enzymatic and microfluidic sensors were also explored for nitrate detection <ref type="bibr">(Xu et al., 2017)</ref>. However, enzyme stability and the complexity of microfluidic settings posed challenges for field use. Nonenzymatic sensors, such as those using differential-pulsed voltammetry or absorption modules, simplified the detection process but required further testing to establish their reliability for field applications <ref type="bibr">(Lu et al., 2025)</ref>. While fiber-optic sensors, field-effect transistors, and spectrophotometric methods offered high precision in nitrate detection, they were often limited by their bulky designs and the need for frequent recalibration <ref type="bibr">(Noman et al., 2022;</ref><ref type="bibr">Xu et al., 2024;</ref><ref type="bibr">Rudd et al., 2017)</ref>. These limitations reduced their practicality for dynamic and long-term field environments. Our sensor coated with the PVA/PSF-PMMA mat showed promise as a practical, inexpensive solution for soil nitrate monitoring under field conditions.</p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head n="4.">Conclusions</head><p>We developed a water-absorbing nanofibrous mat for use in ISEbased soil nitrate sensors. This polymeric mat, composed of PVA, PMMA, and PSF, was fabricated using electrospinning and electrospray techniques. The mat was wrapped around the sensor to draw soil water onto the sensor surface, maintaining a wet state that facilitated the interaction of soil water ions with the sensor. This design addresses a critical issue faced by many existing soil sensors: the lack of waterabsorbing mechanisms for interacting with soil solutions in relatively dry conditions.</p><p>Linear regression analysis of the field measurement results revealed that the mat-wrapped nitrate sensor had a stronger correlation with the salt extract method compared to the bare sensor. This improvement was likely due to the ability of the mat to enhance the presence of soil water and ions at the sensor surface, enabling more representative measurements of soil nitrate levels similar to the conventional method, which analyzed large, homogenized samples. The Bland-Altman analysis revealed that the mat-wrapped sensor exhibited a smaller mean bias and narrower limits of agreement compared to the bare sensor, indicating closer alignment with the conventional salt extract method. Additionally, paired sample t-tests confirmed that the mat-wrapped sensor exhibited improved consistency and lower variability relative to the bare sensor when compared to the conventional method.</p><p>Furthermore, the mat-wrapped sensor performed consistently across varying soil moisture conditions, maintaining a consistent percentage difference with the salt extract method. In contrast, the bare sensor measurements were compromised by changes in soil water content, showing greater variability and less reliability. These findings suggest the mat-wrapped sensor is well-suited for consistent nitrate monitoring across a range of soil moisture levels representative of typical environmental conditions, making it a more viable alternative for robust field applications compared to the bare sensor.</p><p>However, the long-term stability and durability of the mat-wrapped sensor under field conditions remain areas requiring further investigation, particularly regarding microbial activity, wet-dry cycles, soil abrasion, and biodegradability. Deployment in heterogeneous soil environments poses additional challenges, including maintaining consistent sensor-soil particle contact and ensuring uniform water infiltration through the mat. Optimizing the material properties of the nanofibrous mat is critical to enhancing its structural integrity and water-absorbing capacity, thereby improving its effectiveness under field conditions. The biodegradability of the materials used in the mat remains a concern for environmental sustainability. While PVA is partially biodegradable, PSF and PMMA are synthetic polymers with limited degradation in natural environments. Future efforts should focus on integrating bio-based or fully biodegradable materials into the sensor design, ensuring that the hydrophilic properties, mechanical durability, and ion transport efficiency are maintained without compromising performance. Addressing these challenges will necessitate extensive research, involving both controlled experiments and field trials across diverse environmental settings.</p><p>From a system integration perspective, we will focus on integrating the mat-wrapped soil nitrate sensor with soil moisture or water potential sensors, along with energy harvesting technologies <ref type="bibr">(Jiang et al., 2022)</ref>, to improve accuracy, reliability, and longevity for long-term field monitoring. Soil water content significantly affects nitrate sensor readings. Since nitrate ions are highly soluble in water, they move more freely within the soil when moisture levels are higher, leading to a more uniform distribution and easier detection by sensors. In contrast, during dry conditions, nitrate ions may become less mobile and trapped in isolated water films, making them harder to detect and potentially causing inaccurate estimations of nitrate levels. By integrating soil moisture (or water potential) measurements with nitrate monitoring, these variations can be accounted for, resulting in more reliable and consistent detection of soil nitrate levels. Additionally, combining these measurements with subsoil nitrous oxide sensors, which monitor emissions of a potent greenhouse gas <ref type="bibr">(Reay et al., 2012)</ref> will enhance our understanding of soil microbial processes. This integration will provide valuable insights into the interactions between nitrogen availability for plants and nitrous oxide production, supporting the development of more sustainable agricultural practices that balance productivity with environmental stewardship.</p></div><note xmlns="http://www.tei-c.org/ns/1.0" place="foot" xml:id="foot_0"><p>(caption on next page)</p></note>
		</body>