			<titleStmt><title level='a'>A Scalable Methodology for Reinstating the Superhydrophilicity of Ambient-Contaminant Compromised Surfaces</title></titleStmt>
			<publicationStmt>
				<publisher>ACS Publications</publisher>
				<date>04/23/2025</date>
			</publicationStmt>
			<sourceDesc>
				<bibl> 
					<idno type="par_id">10625543</idno>
					<idno type="doi">10.1021/acsami.5c00724</idno>
					<title level='j'>ACS Applied Materials &amp; Interfaces</title>
<idno>1944-8244</idno>
<biblScope unit="volume">17</biblScope>
<biblScope unit="issue">16</biblScope>					

					<author>Ilias Papailias</author><author>Arani Mukhopadhyay</author><author>Anish Pal</author><author>Shahriar Namvar</author><author>Constantine M Megaridis</author>
				</bibl>
			</sourceDesc>
		</fileDesc>
		<profileDesc>
			<abstract><ab><![CDATA[The degradation of the hemiwicking property of superhydrophilic high-energy surfaces due to contaminant adsorption from the ambient atmosphere is well-documented. This degradation compromises the performance of such surfaces, thus affecting their efficacy in real-world applications where hemiwicking is critical. In this work, the role of surface micro-and nanostructure morphology of laser-textured metallic surfaces on superhydrophilicity degradation is studied. We explore intrinsic contact angle variations of superhydrophilic surfaces via the adsorption of organics from the surroundings, which brings about the associated changes in surface chemistry. Furthermore, we explore condensation from humid air as a scalable and environmentally friendly methodology that can reinstate surface superhydrophilicity to a considerable extent (64% recovery of intrinsic wettability after 3 h of condensation) due to the efficient removal of physisorbed contaminants from the surface texture features. The present results strengthen the argument that contact-line movement at fine scales can be used for depinning and removal of adsorbed organic molecules from contaminated surfaces.]]></ab></abstract>
		</profileDesc>
	</teiHeader>
	<text><body xmlns="http://www.tei-c.org/ns/1.0" xmlns:xsi="http://www.w3.org/2001/XMLSchema-instance" xmlns:xlink="http://www.w3.org/1999/xlink">
<div xmlns="http://www.tei-c.org/ns/1.0"><head n="1.">INTRODUCTION</head><p>Hemiwicking (i.e., capillary spreading of a liquid on a rough hydrophilic surface)frequently observed in nature as well as used in technological applicationsis a combined result of surface micro/nanostructures and high surface energy of the underlying solid. <ref type="bibr">1</ref> The wettability of a solid can be quantified by the contact angle of millimeter-diameter water droplets <ref type="bibr">2</ref> or in extreme cases (when the contact angle is too low) by measuring the liquid lateral spreading rate. <ref type="bibr">3</ref> Certain technological applications necessitate the continuous presence of a thin liquid film, as for example in enhanced heat transfer, <ref type="bibr">4</ref> photovoltaic applications, <ref type="bibr">5</ref> maintaining proper thermophysical boundary conditions, <ref type="bibr">6,</ref><ref type="bibr">7</ref> enhanced drainage and collection of a dispersed phase, <ref type="bibr">8</ref> tunable wetting topology, <ref type="bibr">9,</ref><ref type="bibr">10</ref> and the formation of 2D amorphous clathrates. <ref type="bibr">11</ref> Maintaining a thin liquid film on boundary walls of chambers that explore aerosol-cloud-drizzle interactions in a turbulent environment can also be compromised by the degradation examined herein. <ref type="bibr">12,</ref><ref type="bibr">13</ref> Therefore, in such applications, the underlying role of the surface micro/nanotexture of high surface energy materials critically influences not only the wicking rate of liquids (or hemiwicking) <ref type="bibr">14</ref> but also the surface-chemistry interactions. <ref type="bibr">15,</ref><ref type="bibr">16</ref> Among a plethora of methods capable of creating scalable textured surfaces that are also superhydrophilic, <ref type="bibr">[17]</ref><ref type="bibr">[18]</ref><ref type="bibr">[19]</ref><ref type="bibr">[20]</ref><ref type="bibr">[21]</ref><ref type="bibr">[22]</ref> laser ablation has recently gained popularity for efficient surface functionalization, <ref type="bibr">[23]</ref><ref type="bibr">[24]</ref><ref type="bibr">[25]</ref><ref type="bibr">[26]</ref> especially owing to its high microstructure precision, repeatability, and overall scalability.</p><p>During laser ablation, a large amount of energy is released at a prescribed frequency by a pulsed or continuous laser beam, thus creating patterns on (or selectively ablating) a surface. The texture and morphology of the surface patterns are controlled through the laser parameters (beam power, frequency, traversing speed, raster line spacing) that are set in advance of the laser-processing step. By adjusting these laser parameters, different surface architectures can be achieved with high spatial precision and control. As a result of its advantages, laser processing has found its use in several technological applications, ranging from phase-change heat transfer and biology to microfluidics. <ref type="bibr">27</ref> However, the exceptional hydrophilicity and hemiwicking properties of these high-energy surfaces may degrade over time due to adsorption and accumulation of volatile organic compounds (VOCs) during ambient atmosphere exposure (downtime); such adsorption eventually lowers the energy of the surface, thereby turning it hydrophobic, and in turn, compromising its hemiwicking performance. <ref type="bibr">[28]</ref><ref type="bibr">[29]</ref><ref type="bibr">[30]</ref><ref type="bibr">[31]</ref> The most common contamination sources are hydrocarbons that are ubiquitously present in ambient air. <ref type="bibr">32,</ref><ref type="bibr">33</ref> These contaminants can be partially removed from the surface by washing with solvents (e.g., ethanol, acetone, isopropanol, deionized water), or even more effectively, by applying high temperatures (over 180 &#176;C) and complex solvents. <ref type="bibr">34</ref> However, these recovery methods are practically infeasible for large-scale applications, such as convection-cloud chambers, solar thermal desalinators, or falling film evaporators, <ref type="bibr">35</ref> whose surfaces may extend to many square meters. Thus, new approaches that could maintain the continuous wicking functionality of superhydrophilic surfaces and the longevity of their applications must be sought. At the same time, the recovery of superhydrophilicity of exposed surfaces has been rarely studied, as most works up to now have focused on the performance of hydrophobic and superhydrophobic surfaces. <ref type="bibr">[36]</ref><ref type="bibr">[37]</ref><ref type="bibr">[38]</ref><ref type="bibr">[39]</ref><ref type="bibr">[40]</ref> In the present work, the role of surface micro/nanostructure morphology in superhydrophilicity degradation is studied. First, stainless steel surfaces were enhanced with hierarchical microstructures through laser ablation, thus rendering them superhydrophilic. The surfaces were subsequently exposed to a research laboratory open environment, where their superhydrophilicity degraded due to the deposition of VOCs from the air. It has been established that nanofeatures formed on the microstructures during the laser processing step can prevent the accumulation of contaminants on a surface. <ref type="bibr">41</ref> Next, we explored condensation from humid air as a new simple methodology that can reinstate superhydrophilicity and hemiwicking by removing the physisorbed contaminants. In contrast with other methods relying on the use of chemical solvents to dissolve the contaminants from the surface, we explore here a thermophysical method that could restore superhydrophilicity without changing the surface chemistry. Therefore, the novelty of this work lies in understanding how superhydrophilicity of substrates can be recovered by exploiting thermophysical mechanisms, like condensation. The experiments reveal that the combination of molecular desorption at the moving contact line and Laplace pressure differentials during condensate droplet nucleation and growth causes the deposited contaminants to be removed, albeit not completely, from the surface. After exposing surfaces with different texture topologies to the ambient atmosphere for over 8 months, we report convincing evidence that condensation can be more effective in reinstating superhydrophilicity than rinsing with acetone, ethanol, or water. Thus, a new path for scalable and environmentally friendly wettability recovery opens up by establishing surface microstructure design guidelines promoting durable superhydrophilic surfaces.</p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head n="2.">EXPERIMENTAL SECTION</head><p>2.1. Laser Etching Process. 2.1.1. Sample Preparation. SAE 304 stainless steel plates (2 mm thickness) were purchased from</p><p>McMaster-Carr. The plates were composed of a mirror-finished side, which was safely protected by a film. First, the plates were sheared into 3 cm &#215; 3 cm pieces, and the protective film was removed. Then, the samples were sonicated first in deionized water and subsequently in acetone (1 h each) to remove any contaminants from the surface. Next, the samples were subjected to laser ablation. For the scaled-up experiment, a plate of 18 &#215; 26 cm dimensions was sized following the same procedure.</p><p>2.1.2. Laser Ablation. The sample plates were surface-textured via ablation using a 1064 nm nanosecond pulsed 20 W Yb:fiber laser (TYKMA Electrox EMS 300) with a beam spot diameter of 50 &#956;m. The laser parameters used in this study are listed in Table <ref type="table">S1</ref>. The line spacing (i.e., the distance between two adjacent beam raster lines) was the main operational parameter due to its strongest effect on the micro/nanomorphology of the created surface patterns. <ref type="bibr">24</ref> Furthermore, laser-line spacing can affect the cost of the process, as smaller spacings extend the time required for the laser to ablate an area. Each substrate was treated twice: first in one direction and then in another, perpendicular to the original direction. This resulted in an orthogonal cross-hatched microstructure morphology on the surface (Figure <ref type="figure">1</ref>). The sample plates in this work were labeled as SS75, SS125, and SS150 in accordance with the line spacing used to make them (75 &#956;m, 125 &#956;m, and 150 &#956;m, respectively). For the scaled-up experiment, the larger sample (26 cm &#215; 18 cm) was ablated with 150 &#956;m laser-line spacing.</p><p>2.2. Sample Cleansing Process. The cleansing of the surfaces was attained by condensation performed inside an ESPEC SH-641 environmental chamber. The samples were attached to a cold plate (maintained at a temperature of 10 &#176;C) placed vertically inside the chamber to facilitate the downward flow of condensed water due to gravity. The temperature of the chamber was set to 40 &#176;C, and the relative humidity was set to 80%. Each testing cycle lasted for 1 h, after which the surfaces were dried using pure N 2 gas before being characterized. The condensation process was also captured on video using a Canon EOS T1i camera (Supporting Information Video "Condensation"). The amount of water collected during one condensation cycle and the collection rate were also measured, with the results presented in Table <ref type="table">S2</ref>.</p><p>For the rinsing experiment, a Harvard Apparatus PHD ULTRA Syringe Pump was used to create a jet of acetone, ethanol, or water with a flow rate of 50 mL/min (jet velocity 0.3 m/s). The plates were positioned at a 45&#176;angle to maximize the contact with the jet and facilitate the downward flow of the liquid (Supporting Information Video "Rinsing"). After the rinse, the surfaces were dried using pure N 2 gas and subsequently characterized.</p><p>2.3. Water Droplet Spreading Rate Measurements. The spreading rate was quantified by releasing a 4.7 &#956;L water droplet on the prepared surfaces using a syringe (BD) at very low Weber numbers &#8764;O(10 -2 ). The process was recorded at 1000 fps using a Phantom Miro M310 high-speed camera and Phantom Camera Control software. The spreading rate encompasses both the Washburn and Tanner regimes (details in Section S3), thus providing a comprehensive understanding of the transition from capillary-driven infiltration to dissipation-governed spreading, where viscous effects and contact-line dynamics dictate the motion. The original wicking curves are presented in Figure <ref type="figure">S1</ref>. Particular care was taken to eliminate any lingering inertial or neighboring wind effects.</p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head n="2.4.">X-Ray Photoelectron Spectroscopy (XPS).</head><p>The XPS measurements were performed on the prepared surfaces by using a Thermo Fisher Nexsa G2 instrument. Analysis and peak fitting for C, O, and Fe elements were carried out using Thermo Avantage software. All spectra (Figures <ref type="figure">S2-S4</ref>) were calibrated based on the C-C bond binding energy at 284.8 eV.</p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head n="2.5.">Scanning Electron Microscopy-Energy Dispersive Spectroscopy (SEM-EDS).</head><p>High-resolution images and the elemental composition of the prepared surfaces were acquired using a JEOL JSM-IT500HR instrument. The results are presented in Table <ref type="table">S3</ref>.</p><p>2.6. Nanotopology Measurements. The topological characteristics of the surface nanofeatures were studied by using the nanoTOPO-SEM software (Nanometrisis, Greece). Using the acquired high-magnification SEM images, the software analyzes the surface morphology and generates a collection of metrics characterizing the spatial aspects of the surface features (Figures <ref type="figure">S5</ref> and <ref type="figure">S6</ref>).</p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head n="3.">RESULTS AND DISCUSSION</head></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head n="3.1.">Pattern</head><p>Morphology. An orthogonal cross-hatch pattern texture was applied to the stainless steel plates. Parallel trenches were ablated onto the surface, with gaps corresponding to a prescribed line spacing. Thereafter, another set of parallel laser ablation lines perpendicular to the first set was applied on the surfaces. The fine-scale morphology of the created patterns can be seen in the SEM images of Figure <ref type="figure">1A</ref>, <ref type="figure">E</ref>, and <ref type="figure">I</ref>. As expected, the laser acts as a "plow", creating channels of &#8764;50 &#956;m width (consistent with the laser beam spot diameter), while the displaced material is primarily redeposited between these microchannels. Depending on the line spacing used, the area between the microchannels appears either as narrow peaks for the SS75 plate or wide plateaus for the SS125 and SS150 plates. These features can be more clearly observed in the optical profilometry images, where a 3D surface morphology is displayed (Figure <ref type="figure">1D</ref>, <ref type="figure">H</ref>, and <ref type="figure">L</ref>). As revealed in the magnified SEM images (Figure <ref type="figure">1B</ref>, F, and J), after laser ablation, the surfaces are covered with a layer of nanofeatures forming very distinctive, repeatable topologies (Figure <ref type="figure">1C</ref>, <ref type="figure">G</ref>, and <ref type="figure">K</ref>).</p><p>This layer has been previously identified to consist of metal oxide nanoparticles, <ref type="bibr">42,</ref><ref type="bibr">43</ref> produced by oxidation induced by the laser beam and consequent redeposition during laser ablation. <ref type="bibr">[44]</ref><ref type="bibr">[45]</ref><ref type="bibr">[46]</ref> Indeed, the EDS results (Figure <ref type="figure">2</ref>) reveal a significant increase of oxygen from 2.8 at% on an unprocessed stainless steel plate to 25-27 at% on the laser-ablated plates. Interestingly, the nanofeature topology seems to be related to the line spacing. Specifically, the SS75 plate shows the highest abundance of densely packed nanofeatures, while the SS125 and SS150 plates display a sparser distribution.</p><p>3.2. Characterizing Superhydrophilicity after Laser Ablation. The laser-ablated surfaces were superhydrophilic, as total wetting was observed when a 4.7 &#956;L droplet of deionized water was placed at the center of the substrate with minimal impact velocity, Weber number &#8764;O(10 -2 ), to avoid inertial spreading effects. It is well established that the spreading parameter (S) dictates whether a surface gets wetted by a liquid droplet. <ref type="bibr">1</ref> = + S ( )</p><p>where &#947; SV , &#947; SL , and &#947; LV denote the surface energies of the solid-vapor, solid-liquid, and liquid-vapor interfaces, respectively. S &#8805; 0 predicts complete wetting of the substrate by the liquid. Earlier research on droplet spreading behaviors on high-energy substrates has shown that the relevant velocity of the contact line (U) can be modeled from the apparent contact angle (&#952; a ) of the liquid on the surface, under the assumptions of a low Bond number (ratio of the gravitational forces to the surface tension forces), low capillary number, <ref type="bibr">47</ref> and the droplet having the shape of a spherical cap. <ref type="bibr">48,</ref><ref type="bibr">49</ref> These assumptions render the problem one-dimensional, where variations in contact-line velocities at different points along the wetting front can be accounted for by quantifying the wetted area (A) in place of the wetted radius (R). Therefore,</p><p>where &#951; is the liquid viscosity, and m = 3 for liquid spreading (S &gt; 0) on a dry surface. <ref type="bibr">48</ref> Moreover, analysis of the developed microstructures must be carried out in order to distinguish whether the spreading arises from capillarity or hemiwicking through the microstructures. <ref type="bibr">50</ref> Assuming that the Young-Laplace equation &#947; LV cos &#952; = &#947; SV&#947; SL is valid at the contact line and the top of the microstructures remains dry during liquid  imbibition, the critical angle for imbibition (&#952; c ) can be calculated from 51 = r cos 1 c s f s</p><p>where r f denotes the Wenzel roughness, 1 defined as the ratio of the actual surface area to the projected surface area, and &#981; s is the projected solid area fraction that remains dry during the liquid spreading in between the surface asperities. <ref type="bibr">51</ref> The corresponding values of the above quantities along with the average surface roughness (S a ) and intrinsic contact angle (&#952; i ) for the three surfaces are listed in Table <ref type="table">1</ref>. For values of &#952; a &gt; &#952; c , the Wenzel state is attained, where the droplet spreading arises completely due to capillarity through the microstructures. Thus, the intrinsic contact angle (&#952; i ) for the same material with r f = 1 can be estimated from cos &#952; a = r f cos &#952; i . However, in cases where &#952; a &lt; &#952; c , hemiwicking ensues, and an alternate expression, namely cos &#952; a = 1&#981; s (1cos &#952; i ) must be employed. Both of these expressions arise from the hypothesis that for extremely smooth surfaces (where all effects of physical interaction of the liquid with the surface can be neglected), the dynamic contact angles can be assumed equal to the respective static contact angles. Furthermore, estimation of the intrinsic angles on such smooth surfaces (for r f = 1) allows for monitoring how the material surface chemistry changes with VOC adsorption, while neglecting the additional contact-line dynamics or hemiwicking effects arising due to surface micro/ nanotextures. Therefore, extrapolation of the above theory to monitor the contact angle variation with time as VOCs adsorb on the textured surface allows for the estimation of the changes in the underlying physicochemical properties of the surface. <ref type="bibr">1,</ref><ref type="bibr">47</ref> Since the prepared surfaces experience no change in r f during ambient exposure, &#952; i reveals changes in their chemical properties (and thus intrinsic wettability) due to VOC adsorption.</p><p>3.3. Superhydrophilicity Degradation during Ambient Exposure. The superhydrophilicity of the prepared 3 &#215; 3 cm 2 surfaces was examined before and after exposure to a research laboratory environment in Chicago for 1 month (short term) and 8 months (long term). The VOCs in the ambient environment get deposited on the surface, leading to superhydrophilicity degradation of the surfaces, which consequently results in a decreased spreading rate (or hemiwicking). <ref type="bibr">[28]</ref><ref type="bibr">[29]</ref><ref type="bibr">[30]</ref> 3.3.1. Short-Term Exposure. Figure <ref type="figure">3A</ref> shows the spreading rate (mm 2 /s) of a 4.7 &#956;L water droplet deposited on each of the textured surfaces. Soon after fabrication, all the surfaces exhibit a spreading rate of &#8764;400 mm 2 /s, which can be attributed to the similar characteristic width (50 &#956;m) of the created channels and, thus, the exertion of similar capillary forces. <ref type="bibr">52</ref> Our spreading rate aligns with the Lucas-Washburn relation, in agreement with other laser-textured metallic surfaces. <ref type="bibr">2,</ref><ref type="bibr">23,</ref><ref type="bibr">30,</ref><ref type="bibr">31</ref> After 1 week of open-air exposure in the laboratory, the water spreading rate decreases to 170 mm 2 /s for the SS75 plate, 145 mm 2 /s for SS125, and 125 mm 2 /s for SS150. After week 3, a plateau is seemingly reached at 90 mm 2 /s, 75 mm 2 /s, and 65 mm 2 /s, respectively. The superhydrophilicity degradation of the SS75 sample is presented in Figure <ref type="figure">3B</ref> (and Supporting Information Video "Spreading") through the timelapse of a water droplet spreading on the surface before and after 1 month of ambient exposure. The observed degradation can be attributed to the gradual adsorption and accumulation of contaminants on the surface, a phenomenon well established in the literature. <ref type="bibr">29,</ref><ref type="bibr">41,</ref><ref type="bibr">53</ref> XPS measurements were performed on the prepared surfaces before and after exposure to the laboratory environment. The C 1s spectra (Figure <ref type="figure">S3</ref>) show three peaks at 284.8, 286.4, and 288.6 eV, attributed to C-C(H) from hydrocarbon chains or graphitic structures, alcohol/ether C-O groups, and aldehydes/ketones C&#65533;O groups, respectively. <ref type="bibr">54,</ref><ref type="bibr">55</ref> The O 1s spectra (Figure <ref type="figure">S4</ref>) show peaks at 529.8, 531.4, and 533.1 eV, attributed to the Fe-O bonds, the alcohol/ether C-O groups, and the aldehydes/ketones C&#65533;O groups, respectively. <ref type="bibr">54,</ref><ref type="bibr">55</ref> Table <ref type="table">2</ref> shows the carbon (C 1s) and oxygen (O 1s) contents relative to iron (Fe 2p) at different stages of the experiments. The ratio of C 1s to Fe 2p, which indicates the amount of adsorbed organics, <ref type="bibr">56</ref> increased after 1 month of exposure by 80% for the SS75 plate, 92% for SS125, and 100% for SS150. Similarly, the O 1s to Fe 2p ratio increased by 20%, 20%, and 22%, respectively. The XPS results of the degraded surfaces are consistent with VOCs in the Chicago area atmosphere <ref type="bibr">57,</ref><ref type="bibr">58</ref> and directly correlate with the observed decrease of spreading rates. As expected, this change in chemical properties due to VOC adsorption is also reflected in the &#952; i values, which increase after exposure to the ambient environment and then decrease (as superhydrophilicity is recovered) when undergoing condensation from humid air (see sections 3.6 and 3.7). The variation in the extent of &#952; i increase indicates that VOC adsorption is more prominent on the SS150 plate as opposed to SS75 (Table <ref type="table">2</ref>). This trend, observed also during long-term ambient exposure, is attributed to the morphology (or dense packing) of the nanoparticles on the surface. <ref type="bibr">41</ref> Thereafter, the recovery of intrinsic wettability (toward reinstating the smooth-surface chemical properties) was estimated by</p><p>= Recovery 1 i After condensation i Week 0 i Week 4 i Week 0</p><p>thus offering a quantitative criterion for this recovery. Recovery of intrinsic surface wettability (eq 5).</p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head n="3.3.2.">Long-Term</head><p>Exposure. After 8 months of ambient exposure, the surfaces completely lose their superhydrophilicity and hemiwicking properties, thereby exhibiting typical hydrophobic behavior. The deposited water droplet no longer spreads on the surface and instead forms a high static contact angle (&#952; S &gt; 120&#176;) for all plates (Figure <ref type="figure">3C</ref>). Specifically, plate SS75 displays a &#952; S = 137&#176;&#177; 9&#176;, SS125 &#952; S = 146&#176;&#177; 3&#176;, and SS150 &#952; S = 154&#176;&#177; 2&#176;(crossing the widely accepted threshold of superhydrophobicity). It is essential to note that the degree of hydrophobicity is not only dependent on the r f value of the surfaces, which increases with the decreasing line spacing of the laser ablation, but also on the level of VOC adsorption from the environment. Furthermore, the amount of VOCs adsorbed depends on the nanoparticle morphology (size and density) on the top layer of the textured surfaces.</p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head n="3.4.">Examination of Surface Topology.</head><p>The presence and characteristics of surface nanofeatures play a crucial role in the superhydrophilicity degradation (or its reinstatement), as they can dictate the adsorption of contaminants and their diffusion on the underlying surfaces. <ref type="bibr">41,</ref><ref type="bibr">59</ref> Therefore, the formed nanotopology was examined, and the results are presented in Figure <ref type="figure">3D</ref>. As seen in the graph, the average size of nanofeatures and the distance between them greatly vary depending on the beam raster-line spacing. Specifically, the average nanofeature size was calculated (complementary image analysis from SEM micrographs presented in Figures <ref type="figure">S5</ref> and <ref type="figure">S6</ref>) to be 66, 165, and 178 nm for SS75, SS125, and SS150, respectively. <ref type="bibr">60</ref> Similarly, the average distance between these nanofeatures was 38, 100, and 190 nm, respectively. The created nanocavities appear to be characteristic and directly correlated to the superhydrophilicity degradation results. <ref type="bibr">41</ref> We hypothesize that the smaller gaps observed on the SS75 plate significantly inhibit the diffusion of contaminants to the surface, thus slowing degradation caused by the accumulated organics. On the other hand, as the gap between the nanofeatures increases for the SS125 and SS150 samples, higher accumulation of contaminants occurs, resulting in faster wettability degradation. This argument is in line with our hypothesis that a greater nanoparticle density delays the adsorption of VOCs from the ambient environment.</p><p>3.5. Attempting to Reinstate Superhydrophilicity via Rinsing. Earlier exploits in surface cleaning have often adapted rinsing (or washing) the surface with solvents to dissolve the adsorbed VOCs. While some approaches even employ ultrasonication of the substrates in the solvents for increased efficacy, we argue that such an approach would be not only impractical but also infeasible for bigger substrates. Furthermore, ultrasonication is well known for damaging or even removing nanoparticles altogether from the surface, and therefore, it is not suitable in our scenario, where the major objective is to revive the surface wickability while retaining its micro/nanomorphology. Therefore, two methods were adopted for testing the efficiency of removing VOCs from the surface: rinsing and condensation. Rinsing is highly practical owing to its simplicity, and therefore, we washed the surface with common solvents, like acetone, ethanol, and deionized water (Supporting Information Video "Rinsing").</p><p>For long-term exposed plates (Figure <ref type="figure">4B</ref>), rinsing with acetone and ethanol barely improved the wettability for all three samples. Rinsing the surface with deionized water was found to be more effective, as the water contact angle &#952; S on the SS75, SS125, and SS150 plates decreased to 85&#176;, 100&#176;, and 114&#176;, respectively, after 2 h of rinsing. More extended rinsing (a total of 8 h) of the substrates with water followed, where all surfaces turned hydrophilic (15&#176;&lt; &#952; S &lt; 90&#176;). Interestingly, F even such very long durations of washing failed to reinstate the superhydrophilicity and hemiwicking behavior of the surfaces.</p><p>3.6. Reinstating Superhydrophilicity via Condensation. Condensation from warm, humid air in an environmentcontrolled chamber (where a prescribed ambient temperature and relative humidity can be set and maintained) was employed in exploring a non-chemical, environmentally friendly, and scalable methodology for the effective removal of contaminants from ambient-exposed surfaces. The chamber temperature and relative humidity were set to 40 &#176;C and 80%, respectively, whereas the substrate was maintained at 10 &#176;C with the help of an attached cold plate (Section S2).</p><p>Due to the presence of superhydrophilicity-inhibiting VOCs on the surfaces after ambient exposure, condensation occurred in both dropwise and filmwise modes (Figure <ref type="figure">4A</ref>). After an hour-long condensation cycle (measured from the moment when temperature and humidity reached the set values), the wetting ability of the substrates that were short-term exposed was partially recovered. As seen in Figure <ref type="figure">3A</ref>, spreading rates of 240 mm 2 /s, 185 mm 2 /s, and 150 mm 2 /s were measured for SS75, SS125, and SS150, respectively. It is expected that the superhydrophilicity will keep on improving as contact-line movement causes further recovery of the original surface properties via VOC removal.</p><p>In the case of long-term ambient-exposed plates (Figure <ref type="figure">4B</ref>), an hour-long condensation cycle decreased the &#952; S of SS75, SS125, and SS150 plates to 49&#176;, 81&#176;, and 113&#176;, respectively. A subsequent condensation cycle (also for 1 h) further improved the wettability, as the &#952; S of the plates reached 19&#176;, 20&#176;, and 20&#176;, respectively. Therefore, this approach was adopted, and condensation on the samples was continued for 6 more hours (total condensation time of 8 h) until their superhydrophilicity and hemiwicking nature were successfully reinstated. Specifically, the final spreading rate was measured to be 275 mm 2 /s for the SS75 plate, 184 mm 2 /s for SS125, and 105 mm 2 /s for SS150. Although these rates were not comparable to the ones observed before ambient exposure, they were comparable to those observed for the short-term exposed surfaces. Since the cleaning efficiency is dependent on the adhesion between the contaminants and the surface, it is possible that the lack of full recovery can be attributed to chemisorbed contaminants, as both physisorption and chemisorption can occur after lengthy ambient exposure. While "physisorption" refers to the physical adsorption of pollutants onto a surface due to weak forceslike van der Waals interactions -"chemisorption" involves the formation of chemical bonds between the organic contaminants and the functional groups of the surface. <ref type="bibr">61,</ref><ref type="bibr">62</ref> Thus, even organic solvents, such as acetone or ethanol, that can wash off physisorbed contaminants are unable to remove those chemically adsorbed onto a surface through molecular bonds. <ref type="bibr">63,</ref><ref type="bibr">64</ref> An in-depth study of superhydrophilicity reinstatement after physisorbed vs chemisorbed VOCs is beyond the scope of this work.</p><p>3.7. Mechanism for Wettability Recovery. We hypothesize that the recovery in surface superhydrophilicity is attributed to two factors: (1) the nanofeatures serve as preferential nucleation sites during condensation, allowing substantially more time for the contaminants to dissolve into the formed water droplets before they flow downward due to gravity; (2) the moving contact line during condensation can desorb physically adsorbed molecules from inside the nanocavities, enabling "in-depth" cleaning. On the other hand, when simple rinsing is used, the liquid remains in contact with the contaminants for a limited amount of time, and therefore, only the more exposed and easier to dissolve contaminants (i.e., short-chain organics) get removed.</p><p>Earlier experiments on molecular desorption dynamics at the contact line have tied the desorption phenomena predominantly to the movement of the liquid interface over the solid surface. <ref type="bibr">65</ref> High-magnification imaging of the contaminated surfaces during condensation from warm, humid air shows movement of the contact line (Figure <ref type="figure">4A</ref> and Supporting Information Video "Condensation") before a uniform film is formed on the substrate surface. For extremely low capillary numbers (when the contact line either advances or recedes on the surface), such absorbed molecules can be modeled as local chemical heterogeneities. An estimation of the capillary energy (E cap ) for a moving (dynamic) contact line on such local physisorbed surface heterogeneities showed it to be of the order of &#8764;7 k B T, which is comparable to the absorption energy of &#8764;10 k B T per molecule (k B is Boltzmann's constant, and T is the temperature). <ref type="bibr">65</ref> This capillary energy further increases for smaller perimeters of the contact line, thereby supporting the hypothesis that nanoscale features are essential for the "selfcleaning" nature of laser-textured surfaces. Therefore, it is feasible that the contact-line motion provides sufficient energy for the adsorbed molecules to detach from the surface and enter the condensate bulk. Furthermore, we propose that the effect of desorption is magnified when a condensate molecule grows inside a nanostructure pore and is released on the surface. There exist substantial Laplace pressure gradients (noting that the Laplace pressure is inversely proportional to the radius of curvature) from inside the nanopore to millimeter-scale condensate droplets on the surface, which can create significant diffusion gradients for the VOCs to flow out from the micro/nanopores into bigger condensate drops on the surface (Figure <ref type="figure">4C</ref>). The abundance of nanofeatures leads to more nucleation sites during condensation, which allows the generation of more nanodroplets that can participate in the removal of contaminants. This is also evident from the collected amount of condensed water in Table <ref type="table">S2</ref>, which is higher for the SS75 plate and lower for SS125 and SS150. The nucleated nanodroplets experience substantial Laplace pressure differences, which create a strong gradient for adsorbed contaminants to flow out from the surface into the condensate, thus facilitating the observed superhydrophilicity recovery. This is highlighted by the XPS results in Table <ref type="table">2</ref>, where the ratio of C 1s to Fe 2p after condensation is reduced by 24% for the SS75 plate, 18% for SS125, and 16% for SS150 (detailed XPS spectra in Figures <ref type="figure">S2-S4</ref>). Importantly, these values correlate with the observed recovery of spreading rate, with SS75 showing the best recovery among the prepared surfaces.</p><p>3.8. Ramifications for Scaled-Up Applications. The scalability and robustness of the proposed methodology were further tested on a plate with a much larger area (26 &#215; 18 cm) than the original square samples. To ensure that the contamination results are not specific to the Chicago area, the plate was exposed to a research laboratory environment in Houghton, Michigan (Michigan Technological University) for 4 months. After the exposure, the sample was shipped back to Chicago for further testing. Goniometry measurements showed that after ambient exposure, the plates exhibited an average &#952; s of 126&#176;&#177; 9&#176;, with superhydrophilicity completely absent from any part of the surface. Thereafter, the sample was placed on top of a cold plate maintained at 2 &#176;C under typical room conditions (temperature 24-25 &#176;C, relative humidity 38-40%), and condensation was observed (Figure <ref type="figure">5A</ref>). During the process, the ability to maintain a uniform condensation film was tested by locally drying the surface with a jet of pure N 2 (99.999%). As seen in the Supporting Information Video "Condensation-RT", the condensate film quickly recovers to completely cover the substrate, indicating the robustness of the method. After 30 h of continuous condensation, the sample was detached from the cold plate and dried with N 2 , and the hemiwicking properties were characterized with high-speed imaging. Similar to the smaller samples, the superhydrophilicity was fully reinstated after condensation, with the plate showing a spreading rate of 295 mm 2 /s (Figure <ref type="figure">5B</ref>).</p><p>These results prove the scalability of the condensation cleansing method and highlight that: (1) the approach is effective, regardless of the geographical location where a surface is exposed; (2) there is no need for extreme condensation conditions, as normal (room) temperature and humidity values would suffice.</p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head n="4.">CONCLUSIONS</head><p>Superhydrophilic stainless steel surfaces were produced by surface texturing using nanosecond pulsed laser ablation. The superhydrophilicity degradation due to the accumulation of VOCs from ambient exposure and the subsequent reinstatement via condensation from humid air were studied. It was revealed that the nanofeature topology has a significant impact on the wettability loss of the surfaces and its recovery. The results indicate that the formation of narrow nanocavities inhibits the diffusion of contaminants and prevents their accumulation on the underlying solid. When these nanocavities are wider, the deposited organic layer penetrates the underlying surface, thus leading to accelerated degradation and less efficient recovery. Besides controlling the deposition of the VOCs on the underlying surface, the nanofeatures also significantly affect the recovery through condensation. The nucleating nanodroplets on the nanofeatures experience substantial Laplace pressure differences, which ultimately create a strong gradient for contaminants to be removed from the surface and into the condensate. Furthermore, the moving contact line desorbs molecules that were physically adsorbed to the surface, facilitating VOC removal and therefore "cleansing" at the nanoscale level. Due to these phenomena, condensation proves to be more efficient than chemical rinsing with acetone, ethanol, or water and thus emerges as a promising scalable and environment-friendly alternative methodology for reinstating hemiwicking on a textured superhydrophilic surface without altering its micro/ nanosurface morphology.</p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head>&#9632; ASSOCIATED CONTENT</head></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head>* s&#305; Supporting Information</head><p>The Supporting Information is available free of charge at <ref type="url">https://pubs.acs.org/doi/10.1021/acsami.5c00724</ref>. </p></div><note xmlns="http://www.tei-c.org/ns/1.0" place="foot" xml:id="foot_0"><p>https://doi.org/10.1021/acsami.5c00724 ACS Appl. Mater. Interfaces XXXX, XXX, XXX-XXX B</p></note>
			<note xmlns="http://www.tei-c.org/ns/1.0" place="foot" xml:id="foot_1"><p>https://doi.org/10.1021/acsami.5c00724 ACS Appl. Mater. Interfaces XXXX, XXX, XXX-XXX C</p></note>
			<note xmlns="http://www.tei-c.org/ns/1.0" place="foot" xml:id="foot_2"><p>https://doi.org/10.1021/acsami.5c00724</p></note>
			<note xmlns="http://www.tei-c.org/ns/1.0" place="foot" xml:id="foot_3"><p>https://doi.org/10.1021/acsami.5c00724 ACS Appl. Mater. Interfaces XXXX, XXX, XXX-XXX G</p></note>
			<note xmlns="http://www.tei-c.org/ns/1.0" place="foot" xml:id="foot_4"><p>https://doi.org/10.1021/acsami.5c00724 ACS Appl. Mater. Interfaces XXXX, XXX, XXX-XXX H</p></note>