<?xml-model href='http://www.tei-c.org/release/xml/tei/custom/schema/relaxng/tei_all.rng' schematypens='http://relaxng.org/ns/structure/1.0'?><TEI xmlns="http://www.tei-c.org/ns/1.0">
	<teiHeader>
		<fileDesc>
			<titleStmt><title level='a'>A mechanistic powder compaction equation: Accounting for the effects of particle properties</title></titleStmt>
			<publicationStmt>
				<publisher>Elsevier</publisher>
				<date>10/01/2025</date>
			</publicationStmt>
			<sourceDesc>
				<bibl> 
					<idno type="par_id">10664839</idno>
					<idno type="doi">10.1016/j.powtec.2025.121285</idno>
					<title level='j'>Powder Technology</title>
<idno>0032-5910</idno>
<biblScope unit="volume">464</biblScope>
<biblScope unit="issue">C</biblScope>					

					<author>Zhixing Lin</author><author>Christopher Kossor</author><author>Liang Chen</author><author>Rajesh Davé</author>
				</bibl>
			</sourceDesc>
		</fileDesc>
		<profileDesc>
			<abstract><ab><![CDATA[Not Available]]></ab></abstract>
		</profileDesc>
	</teiHeader>
	<text><body xmlns="http://www.tei-c.org/ns/1.0" xmlns:xsi="http://www.w3.org/2001/XMLSchema-instance" xmlns:xlink="http://www.w3.org/1999/xlink">
<div xmlns="http://www.tei-c.org/ns/1.0"><head n="1.">Introduction</head><p>The development of pharmaceutical tablets has witnessed significant advancements over the years, with the extensive use of tablets playing a pivotal role in this evolution <ref type="bibr">[1]</ref><ref type="bibr">[2]</ref><ref type="bibr">[3]</ref>. Tablet hardness, a critical parameter in tablet quality assessment, serves as a key indicator of a tablet's mechanical integrity and can be further quantified as tensile strength, dependent on the tablet's dimensional characteristics. Traditionally, tablet formulation has relied on a trial and error approach to enhance tablet tensile strength <ref type="bibr">[4,</ref><ref type="bibr">5]</ref>. However, there is a need to move beyond trial-and-error (empirical) methods. By adopting science-based, predictive approaches, drug development can become faster, less costly, and more reliable, thus potentially facilitating more rapid clinical trials, smoother regulatory approval, and lesser manufacturing failures.</p><p>The discussion surrounding factors influencing tablet tensile strength has been extensive, and numerous models have been developed to empirically describe this crucial property <ref type="bibr">[6]</ref><ref type="bibr">[7]</ref><ref type="bibr">[8]</ref><ref type="bibr">[9]</ref><ref type="bibr">[10]</ref>. Ryshkewitch and Duckworth (RD) introduced the tablet porosity (&#949;) and tablet tensile strength (&#963;) equation Eq. ( <ref type="formula">1</ref>) <ref type="bibr">[6]</ref> to assess the compactability of a material.</p><p>The RD compactability relationship indicates that the tablet tensile strength, &#963;, decays exponentially from the zero-porosity tensile strength, &#963; 0 , as described by the experimentally determined decay constant, k RD .</p><p>Although the RD equation lacks a comprehensive physical explanation of how particle properties precisely affect tablet tensile strength, various mixing rules have been integrated into the equation, allowing predictions to extend from single-component to binary-component systems <ref type="bibr">[11,</ref><ref type="bibr">12]</ref>. Furthermore, an array of empirical tablet porosity prediction models can be utilized to refine tensile strength predictions based on the RD equation <ref type="bibr">[8,</ref><ref type="bibr">[13]</ref><ref type="bibr">[14]</ref><ref type="bibr">[15]</ref><ref type="bibr">[16]</ref><ref type="bibr">[17]</ref>. However, even with these advancements, a fundamental understanding of particle interactions and tablet formation remains elusive. In addition to the RD equation, researchers have examined the influence of surface energy on tensile strength under specific conditions, controlling particle size and tablet thickness <ref type="bibr">[18,</ref><ref type="bibr">19]</ref>. The concept of bonding strength and bonding number, introduced by Eriksson and Alderborn in 1995 <ref type="bibr">[20]</ref> and subsequently elaborated upon by Sun in 2011 <ref type="bibr">[21]</ref>, represents a significant development in understanding tablet properties. Recently, a new empirical equation was established to predict the tabletability profiles of powders by elegantly combining the RD compactability equation and the Kuentz-Leuenberger (KL) compressability Eq. <ref type="bibr">[22]</ref>.</p><p>The KL compressability equation (Eq. ( <ref type="formula">2</ref>)) relates the compaction pressure, P, and tablet porosity, &#949;, with a critical tablet porosity, &#949; c , and a powder plasticity term 1 C . Despite these advancements, there currently exists no practical equation that transcends empirical correlations describing bonding strength and bonding number based on interparticle interactions and tablet dimension. This represents a crucial research gap in the field of tablet development and necessitates further investigation.</p><p>The primary objective of this study is to quantitatively assess and validate the concept of bonding strength and bonding number. To achieve this, the study will adapt a particle adhesion force model for calculating bonding strength and employ a particle coordination number approach to calculate bonding number, which is the number of contacts at cross-section. By leveraging the properties of the particles and specific tablet dimensions, the study aims to establish formulation guidelines. The proposed model is expected to serve as a valuable resource, offering guidance for rational excipient design, rational formulation design, and in subsequent work, estimates of the highest possible drug loading. Ultimately, this mechanistic model intends to provide a comprehensive and practical framework for quantifying and predicting tablet tensile strength, thus offering valuable insights for tablet design and pharmaceutical formulation.</p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head n="2.">Materials and methods</head></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head n="2.1.">Materials</head><p>Microcrystalline cellulose, Avicel PH-101 (AV101), Avicel PH-102 (AV102), and Avicel PH-105 (AV105) were denoted by FMC Corporation (St. Louis, MO, USA). Mannitol, Mannogem Powdered 112-1239 (Mannitol 1239) and 112-1194 (Mannitol 1194) were donated by SPI Pharma Inc. (Wilmington, DE, USA).</p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head n="2.2.">Particle sizing via laser diffraction</head><p>The mean particle size, D 50 and Sauter Mean Diameter D 3,2 was measured by utilizing Sympatec Helos/Rodos laser diffraction particle size analyzer (Sympatec Inc., NJ) at the dispersion pressure of 1.0 bar, the dispersion pressure which resulted in the most consistent particle size distribution measurements as other studies prove <ref type="bibr">[23,</ref><ref type="bibr">24]</ref>. Particle size distribution values are summarized in Table <ref type="table">1</ref>. It is noted that laser diffraction techniques estimate particle size distribution without accurately accounting for actual particle shape and cannot distinguish coarse and fine non-spherical particles well.</p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head n="2.3.">Tablet compression</head><p>All materials were compacted in a Gamlen D1000 (Gamlen Tableting Ltd., London, UK) compactor to prepare 100 mg cylindrical, flat-faced tablets, utilizing a 6 mm punch die. There were 9 compaction loads applied, and five tablets were compacted at each load.</p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head n="2.4.">Tablet tensile strength</head><p>The tablet diameter and breaking force was measured (n = 5) from a diametrical compression test with a Texture Analyzer (Texture Technologies Corp., USA). A Gamlen TTA (Gamlen Tableting Ltd., London, UK) was used to assess the tablet diameter and breaking force via a diametrical compression test (n = 5). The tablet tensile strength was computed by Eq. (3) <ref type="bibr">[25]</ref> was applied to calculate the tensile strength for each formulation and compaction force. In the equation, &#963; is the tensile strength, F t is the tablet breaking force, D t is the tablet diameter, and t is the thickness of the tablet.</p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head n="2.5.">Tablet porosity</head><p>The powder true density (&#961; t ) was characterized by a Pycnometer (NOVA 3200, Quantachrome Instruments, Boynton Beach, FL, USA) with Helium gas. This experiment was conducted five times, and the average values are reported in Table <ref type="table">1</ref>. The tablet porosity (&#949;) was evaluated by comparing the tablet density (&#961;) and the particle true density as shown in Eq. ( <ref type="formula">4</ref>),</p><p>where m is mass of tablet.</p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head n="2.6.">Surface energy</head><p>Surface energy was evaluated using automated inverse gas chromatography (SEA-IGC; Surface Energy Measurement System Ltd., UK) via the Schultz method <ref type="bibr">[26]</ref>. Detailed description of sample preparation and surface energy evaluation may be found elsewhere <ref type="bibr">[27]</ref>.</p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head n="3.">Theory</head></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head n="3.1.">Bonding strength and bonding number</head><p>The presence of particles in a tablet can be expressed as strong agglomerations of particles that interact strongly with each other. Therefore, the breaking force of a fracture plane can be derived from the product of the individual bonding strength between particles and the number of all bonds in the plane of the fracture plane <ref type="bibr">[28,</ref><ref type="bibr">29]</ref> as shown in Fig. <ref type="figure">1</ref> and described in Eq. <ref type="bibr">(5)</ref>.</p><p>Where F t is the force to fracture the tablet, N is number of particle bonds on the cross-plane (bonding number), and F p is bonding strength between two particles. This approach assumes that the fracture plane breaks instantaneously within the tablet cross-sectional area and that voids are evenly distributed to ensure applied compression pressure is evenly distributed on the cross section. Evaluating the right-hand side of Eq. ( <ref type="formula">4</ref>) requires a profound understanding of particle properties such as bonding strength and bonding number.</p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head n="3.2.">Bonding strength</head><p>Bonding strength can be viewed as the adhesion force between two particles. Rumpf's adhesion equation (Eq. ( <ref type="formula">6</ref>)) is one of the formulas that elucidates the adhesion force between two particles without compression <ref type="bibr">[30]</ref>.</p><p>Where F ad is adhesion force of the powder material between two particles, A H is the Hamaker constant, D 3,2 is the Sauter diameter of the particle, z 0 is the equilibrium separation distance of 0.4 nm <ref type="bibr">[31]</ref><ref type="bibr">[32]</ref><ref type="bibr">[33]</ref>, D 0 is the cut-off distance as 0.165 nm <ref type="bibr">[34]</ref>, and &#947; is the particle surface energy.</p><p>Following compression, the anticipated outcome is the increase of contact area between particles, resulting in an greater bonding strength <ref type="bibr">[21]</ref>. It is reasonable to assume that bonding strength can be represented by interparticle adhesion force after compression and is directly proportional to the contact area <ref type="bibr">[35]</ref>. The calculation of contact area after compression necessitates a thorough understanding of particle consolidation. Assumptions based on material properties are presented in Fig. <ref type="figure">2</ref> to illustrate the contact between particles during compression.</p><p>Hence, when powder is subjected to compression, the contact radius, a, is calculated using Eq. ( <ref type="formula">8</ref>), by incorporating previously established contact models <ref type="bibr">[36,</ref><ref type="bibr">37]</ref>. The contact radius is linearly dependent on the initial contact radius, a 0 , before compression and the product kP 1 3 where k denotes the brittle property and P is the loading pressure <ref type="bibr">[37,</ref><ref type="bibr">38]</ref>.</p><p>Eq. ( <ref type="formula">9</ref>) defines the initial contact radius where, &#947; is the surface energy     <ref type="formula">2</ref>)) was inverted to define porosity as a function of pressure to adapt the general model (Eq.( <ref type="formula">17</ref>)) for tabletability prediction.</p><p>of the material, v is the Poisson's ratio, E, is the characteristic Young's Modulus, and r, is the characteristic radius. The characteristic value, X, is evaluated by</p><p>where X 1 and X 2 are placeholders for a particle property of particle 1 and particle 2, respectively. In practice, the brittleness of the material determines the type of deformation that occurs during compression. Brittle materials, characterized by a reduced tendency to deform, exhibit asperity-level (local) deformation rather than particle-level deformation under compression pressure. Conversely, for ductile materials, particle-level deformation takes precedence over asperity-level deformation. The contact radius remains constant during compression, while the particle experiences a higher number of asperity contacts due to its plastic properties. Note, if the material is ductile, then the brittle property, k, can be assumed to be zero, but if the material is brittle, then k needs to be calculated.</p><p>The bonding strength, F p , is scaled proportionally to the ratio of initial and final contact areas expressed as, <ref type="bibr">(10)</ref> Where A represents the contact area between two particles without pressure (assumed as a constant), and A &#697; is contact area between two particles after compression which can be described by c &#697; &#960;a 2 , where c &#697; signifies the number of contact points or number of asperities that contact a neighboring particle after compression. For simplification, let c represent the corrected contact number, c &#697; &#960; A . Corrected contact number can also be described as the scaling factor of adhesion force from before compression to after compression that arises due to te increased contact area between particles, thus combining Eqs. (6-10), bonding strength is expressed in Eq. <ref type="bibr">(11)</ref>.</p><p>] 2 A H D 32 12z 0 2 (11)</p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head n="3.3.">Bonding number</head><p>Bonding number, denoted as N, is the number of interparticle bonding per cross-sectional area, as illustrated in Fig. <ref type="figure">3</ref> and expressed by the product of the coordination number (n c ) and the number of particles in the cross-section fracture plane (n F ). The coordination number (n c ) of one particle is <ref type="bibr">[39]</ref> is expressed by n c = &#960; &#949; where &#949; is the porosity of the tablet. To calculate particle numbers on the tablet cross-plane (n F ), it is assumed that tablet breaks across the diameter of the tablet cross sectional area, A c ,</p><p>where D t is the tablet diameter, and t is the thickness of the tablet.</p><p>The area of the fracture plane of a compact is estimated as A c (1 -&#949;) <ref type="bibr">[40]</ref>. However, the fracture plane may not contain the diameter of all particles, thus the mean projected particle area must be taken into consideration. The particles in the cross-section are assumed to be spherical and the quantity in the cross-section (n F ) can be estimated by the ratio of cross-section area to the mean projected particle area (f m ),</p><p>where D 50 is the particle size of powder, z is the distance from center of particle to the plane at which the particle is cut off by the cross-section.</p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head n="3.4.">A mechanistic powder compaction equation</head><p>Now, the breaking force (F t ) can be expressed by combing Eqs. 11 and 15,</p><p>Thus, the expression for the tensile stress of the tablet is shown in Eq. ( <ref type="formula">17</ref>) by combining Eqs. ( <ref type="formula">3</ref>) and ( <ref type="formula">16</ref>) to normalize the breaking force with the tablet dimensions,</p><p>where F ad is defined in Eq. ( <ref type="formula">6</ref>).</p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head n="3.5.">Applying the compaction equation</head><p>The corrected contact number, c, and brittle property term, k, must be determined experimentally by comparing the actual tablet tensile stress, &#963;, in Eq. ( <ref type="formula">3</ref>) to the intermediate predicted tablet tensile stress, &#963;t c , for each compaction pressure along with the porosity in Eq. ( <ref type="formula">17</ref>). In practice, c is the ratio of &#963;t &#963; for the tablet made of a given powder material. The experimental data can be fit globally across the pressure and porosity ranges such that a single c and k value is determined per material and per particle property. For example, for a given material with 3 particle sizes, then there would be 3 sets of c and k parameters. A novelty of the presented compaction equation is that it can be adapted model both: tabletability (&#963; -P) and compactability (&#963; -&#949;) since it simultaneously requires pressure and porosity as seen in Eq. ( <ref type="formula">17</ref>). The compaction equation Eq. ( <ref type="formula">17</ref>) can be combined with an established compressability (&#949; -P) equation <ref type="bibr">[13,</ref><ref type="bibr">15,</ref><ref type="bibr">16,</ref><ref type="bibr">41]</ref>, like the KL equation (Eq. ( <ref type="formula">2</ref>)), to substitute the &#949; term for &#949;(P) via the KL equation to write Eq. ( <ref type="formula">17</ref>) as a tabletability equation or substitute the P term for P(&#949;) via the KL equation to write Eq. ( <ref type="formula">17</ref>) as a compactability equation.</p><p>Nonlinear regression of the tabletability and compactability data to Eq. ( <ref type="formula">17</ref>) was performed in Python (v3.12.3) using SciPy's (v1.13.1) least squares trust region reflective algorithm. The required particle properties are included in Table 1 <ref type="bibr">[42]</ref><ref type="bibr">[43]</ref><ref type="bibr">[44]</ref>.</p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head n="4.">Results and discussion</head></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head n="4.1.">Sensitivity analysis of mechanistic parameters</head><p>The advantage of this mechanistic based model is to quantify parameters within the tableting process instead of relying upon several empirical parameters that lead to inferior trial and error type of approach. Critical particle properties necessary for this model include mean particle size, Sauter mean diameter, surface energy, Young's modulus (modulus), corrected contact number, and particle brittle properties. The former 4 parameters influence the corrected contact number and the brittle property. Each of these parameters has been investigated with sensitivity analysis and summarized in Fig. <ref type="figure">3</ref> for tabletability and Fig. <ref type="figure">4</ref> for compactability with a set of constant base parameters that were maintained for each subplot. Another novelty of this model is demonstrated by the ability to vary system parameters such as particle size distribution for a given material and develop a mechanistic understanding of the powder compaction profiles. Thus, this can aid in determining the optimal particle size for the desired tablet mechanical properties. For example, Fig. <ref type="figure">3a-b</ref> and Fig. <ref type="figure">4a-b</ref> demonstrate that for a fixed modulus, Poisson's ratio, and surface energy, the tablet tensile strength can be predicted for a range of particle sizes. The surface energy has a subtle influence on the predicted powder compaction profiles evident by profiles depicted in Fig. <ref type="figure">3c</ref> and Fig. <ref type="figure">4c</ref> since it only affects the interparticle adhesion force (Eqs. ( <ref type="formula">6</ref>) and ( <ref type="formula">7</ref>)) and the initial contact radius (Eq. ( <ref type="formula">9</ref>)). The material modulus has nearly a negligible impact on tensile strength when plotted for values ranging from 7 to 11GPa shown by nearly the same curves in Fig. <ref type="figure">3d</ref> and Fig. <ref type="figure">4d</ref>. Lastly, a range of corrected contact numbers and brittle property are shown in Fig. <ref type="figure">3e-f</ref> and Fig. <ref type="figure">4e-f</ref>.</p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head n="4.2.">Model validation: ductile materials, k = 0</head><p>The predicted breaking force is directly proportional to the adhesion force among neighboring particles and ratio of the contact area after to before compression (Eq. ( <ref type="formula">10</ref>)). The surface area after compression can be calculated knowing the contact radius a (Eq. ( <ref type="formula">8</ref>)); however, the initial surface area cannot directly be estimated since the contact number before compression c &#697; is not explicitly defined and is condensed into the corrected contact number, c. Thus, c can be determined for a material of a known particle size at range of pressures to predict the tabletability or compactability of additional particle sizes and or porosities for the same material. It is assumed that the class of ductile materials effectively results in no direct pressure contribution to the contact surface are as seen in Table <ref type="table">2</ref> by when k = 0 in Eq. ( <ref type="formula">8</ref>), thus the only contributions of pressure to the predicted tensile strength is through the compressibility relationship with porosity.</p><p>Each MCC grade resulted in increased tensile strength with rising compaction pressure and closely aligned with the experimental tensile strength after c was determined. The prediction tends to deviate at lower porosity values and this discrepancy could be attributed to the incapability of parameter c for capturing powder compaction behavior at low porosity. When a breaking force is applied to the tablet, it fractures from the weakest or most porous section, resulting in a breaking force lower than predicted <ref type="bibr">[45]</ref><ref type="bibr">[46]</ref><ref type="bibr">[47]</ref>.</p><p>The utility of this adhesion force-based tablet strength model was demonstrated by evaluating a wide range of particle sizes and tablet porosities to highlight the novel predictive capabilities of the corrected contact number, c. The tabletability (&#963; -P) curves were constructed by evaluating the tensile strength for a range of loading pressures (Fig. <ref type="figure">5</ref>) each MCC grade. The compactability (&#963; -&#949;) curves were constructed by evaluating the tensile strength for a range of corresponding tablet porosities (Fig. <ref type="figure">6</ref>) for each MCC grade. It should be noted that when tablet porosity is &lt;0.15, tablet tends to be under over compaction. It is out of scope of this mechanistic model; therefore, this model may not precisely predict it, although it works for each MCC grades.</p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head n="4.3.">Model validation: brittle materials, k &#8725; = 0</head><p>In contrast to ductile materials, the class of brittle materials do not eliminate the pressure contributions to the contact surface are in Eq. ( <ref type="formula">8</ref>), thus k &#8725; = 0 (Table <ref type="table">2</ref>). In practice, this yields that the corrected contact  <ref type="formula">2</ref>)) was used to define pressure as a function of porosity to adapt the general model (Eq. ( <ref type="formula">17</ref>)) for compactablity prediction. number, c, and the brittle property, k, must be found simultaneously for a given material and particle properties. As illustrated in Fig. <ref type="figure">2</ref>, the hypothesis is that when compaction pressure increases, ductile material tends to yield or deform leading to particle level deformation rather than asperity level deformation (local deformation) due to its ductile nature. The brittle material, which has low tendency to deform, suffering high compaction pressure, tends to perform asperity level deformation. It contributes to contact area by increased contact radius. This hypothesis well describes the existence of the term of brittle property, k, and it contributes to quantify increased contact area during compaction. Two grades of Mannitol, 1239 and 1194, were selected to investigate the impact of the brittle property on the predicted tensile strength. In Table <ref type="table">2</ref>, the brittle property term, k, increased from 9.54 &#215; 10 accordance with the asperity level deformation assumption. As the k parameter describes the asperity level deformation, that is more likely to be determined by asperity property or asperity size. Correspondingly, different grades of Mannitol are likely to have different asperity properties as size changes. While diverse sizes of Mannitol data may be necessary to validate the trend, it appears that smaller size leads to a smaller k value. Besides, based on definition of brittle property term, k, which refers to asperity level deformation, it is noted that k value of ductile material is 0. That indicates that with increasing particle size, Mannitol tends to be more brittle. Thus, the parameter k is likely to provide a new way to describe the property of an excipient.</p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head n="4.4.">Effect of particle size on corrected contact number</head><p>The corrected contact number, c, is an extrinsic property since the particle size and porosity can influence its value. The relationship of MCC between particle size and the average corrected contact number is shown in Fig. <ref type="figure">7</ref>. As particle size decreased, the c of MCC (Table <ref type="table">2)</ref>   represent greater fragmentation: hence, a larger contact area between particles. These findings suggest that the corrected contact number, c, can represent the extent of surface contact between two particles and provide insight into a mechanistic understanding of tablet compaction and fracture. It should be noted that corrected contact number of Mannitol is four magnitudes smaller than MCC, which indicates that local deformation led to higher contact area than fragmentation.</p><p>Ultimately, the principal goal of this tabletability equation is to mechanistically guide the design of a single component compacted tablet. The tabletability surface can be predicted as shown in Fig. <ref type="figure">8</ref> for three MCC grades. The surface can be generated by explicit physical parameters, most notably particle size and tablet porosity, by only using experimental tablet porosity and tensile strength from three MCC grades spanning from 19 to 117 &#956;m. Thus, mechanistic insight can be gained during tablet formulation by providing direct access to interparticle interactions for a given material to the prediction of tablet strength.</p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head n="4.5.">Assumptions, limitations, and future direction of the model</head><p>The tableting system in this study is simplified into a single component tablet to isolate the fundamental mechanisms of compaction behavior. The model does not consider elastic and resilient situations hence the tablet dimensions used are out-of-die measurements. The predictability of the model spans both brittle and ductile materials. Fragmentation is one of the characteristics of brittle materials. It is assumed that fragments of one particle are consolidated into a new particle with similar particle size but in different shapes after compression. Under that assumption, the differences between the original particle and fragmented-and-consolidated particle are reflected in the increased bonding number and contact area, which is compensated by our bonding number and corrected contact number, respectively.</p><p>The major limitation of this model is that the corrected contact number is only approximately constant under certain compaction range, most likely between 100 MPa to 300 MPa. When compaction pressure is low, particles do not fully contact each other leading to reduced corrected contact number. Hence, it leads to an overestimate of tensile strength at low compaction pressure. While compaction pressure is high, low porosity leads to complete contact between two particles. Merger between two particles may happen, and it could lead to unpredictable changes in tablet tensile strength. It is recommended that this model should be used for solid fractions in range 0.6-0.85. This model is expected to facilitate prediction of compaction for binary and multi-component blends through a mechanistic mixing rule, which would be the subject of the subsequent paper. Such model may offer theoretical calculation of tablet tensile strength based on formulation, tablet dimension, and properties of individual components, thereby reducing reliance on empirical experimentation.</p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head n="5.">Conclusion</head><p>The proposed mechanistic model is shown to provide insight into the interplay of particle properties that contribute to tablet tensile strength by incorporating material properties with two fitting parameters. The tablet tensile strength is modeled by two overall terms: bonding number and bonding strength. The model incorporates mechanistic particle properties including primary particle size, Sauter mean diameter, surface energy, Young's modulus, and Poisson's ratio to calculate the bonding strength and bonding number with tablet porosity and compaction pressure. The bonding strength is derived from the interparticle adhesion force and the asperity contact radius under compression. The bonding number is derived from the coordination number and number of particles in the fracture plane. The two fitting parameters, brittle parameter k and corrected contact number c are related to powder brittleness tendency and contact area after compression, respectively that govern the required tablet breaking force. For ductile materials, the value of k is zero (0), thus the asperity contact radius remain constant, independent of compaction pressure. For brittle materials, brittle parameter k represents the extent of change in local asperity shape at the contact point. Corrected contact number c is strongly related to particle-particle bonding strength and its value represents the number of asperity bonds between particles, thus the correct contact number is strongly inversely correlated to the primary particle size. This investigation illustrates the impact of six critical parameters include powder material size, represented by mean particle size and Z. Lin et al. Powder Technology 464 (2025) 121285</p><p>Sauter mean diameter, tablet porosity, surface energy, Young's modulus, corrected contact number, and particle brittle properties; predictive capabilities of the model based on three size grades of MCC and two size grades of Mannitol; and extends to a range of theoretical particle sizes and tablet porosities based on the material properties of MCC. Thus, this study provides a novel mechanistic powder compaction model that provides insight into excipient design and the potential for tablet formulation design.</p></div></body>
		</text>
</TEI>