			<titleStmt><title level='a'>Open-Air Growth of Polymer Brushes by Surface-Initiated PhotoATRP under Red-Light Irradiation</title></titleStmt>
			<publicationStmt>
				<publisher>ACS</publisher>
				<date>07/02/2025</date>
			</publicationStmt>
			<sourceDesc>
				<bibl> 
					<idno type="par_id">10692397</idno>
					<idno type="doi">10.1021/acsami.5c08584</idno>
					<title level='j'>ACS Applied Materials &amp; Interfaces</title>
<idno>1944-8244</idno>
<biblScope unit="volume">17</biblScope>
<biblScope unit="issue">26</biblScope>					

					<author>Yuwen Zhang</author><author>Alessio Lo Bocchiaro</author><author>Xiaolei Hu</author><author>Carlos Pavon</author><author>Cristian Pezzato</author><author>Krzysztof Matyjaszewski</author><author>Francesca Lorandi</author><author>Edmondo M Benetti</author>
				</bibl>
			</sourceDesc>
		</fileDesc>
		<profileDesc>
			<abstract><ab><![CDATA[Not Available]]></ab></abstract>
		</profileDesc>
	</teiHeader>
	<text><body xmlns="http://www.tei-c.org/ns/1.0" xmlns:xsi="http://www.w3.org/2001/XMLSchema-instance" xmlns:xlink="http://www.w3.org/1999/xlink">
<div xmlns="http://www.tei-c.org/ns/1.0"><head n="1.">INTRODUCTION</head><p>Translation of polymer brushes into technologically relevant coating materials requires robust and scalable fabrication processes, which necessarily encompass the development of surface-initiated controlled polymerization techniques that can be easily performed within industrially relevant settings.</p><p>Surface-initiated reversible deactivation radical polymerizations (SI-RDRPs) represent the major class of techniques for synthesizing polymer brushes, giving access to a broad variety of functional brush coatings with fine control over polymer structural parameters, including thickness (i.e., molar mass), dispersity (&#272;), grafting density (&#963;), and polymer architecture/topology. <ref type="bibr">1</ref> Among the main requirements for developing SI-RDRP processes that are compatible with the large-scale synthesis of brushes, a high tolerance toward environmental conditions is probably the most stringent. <ref type="bibr">[2]</ref><ref type="bibr">[3]</ref><ref type="bibr">[4]</ref><ref type="bibr">[5]</ref> Processes that are compatible with nondegassed reaction mixtures and/or exposure to the environment permit a steady brush growth while avoiding radical recombination with molecular oxygen. To this aim, different SI-RDRP techniques have been developed, typically exploiting oxygen scavengers present in the polymerization mixture, including zerovalent metals, <ref type="bibr">[6]</ref><ref type="bibr">[7]</ref><ref type="bibr">[8]</ref><ref type="bibr">[9]</ref> sacrificial catalysts/ cocatalysts, <ref type="bibr">[10]</ref><ref type="bibr">[11]</ref><ref type="bibr">[12]</ref><ref type="bibr">[13]</ref> and enzymes. <ref type="bibr">14,</ref><ref type="bibr">15</ref> Among the SI-RDRP techniques that show a certain tolerance toward oxygen, light-mediated processes have greatly surged in recent years, <ref type="bibr">[16]</ref><ref type="bibr">[17]</ref><ref type="bibr">[18]</ref> including surface-initiated photoinduced atom transfer radical polymerization (SI-photoATRP) and surface-initiated photoinduced electron/energy transfer reversible addition-fragmentation chain-transfer (SI-PET-RAFT) polymerization. These versatile processes have been employed to fabricate a vast range of materials, including polymeric bioconjugates and 3D-printed nanostructured materials. <ref type="bibr">19,</ref><ref type="bibr">20</ref> In an analogous way to the corresponding solution process, SI-photoATRP is typically performed under UV light irradiation. <ref type="bibr">11,</ref><ref type="bibr">21,</ref><ref type="bibr">22</ref> During this process, ATRP deactivators XCu II L + (X = Br or Cl, and L is a multidentate amine ligand) are photoexcited upon absorbing light and subsequently reduced by an electron donor&#65533;usually uncoordinated L present in an excess&#65533;to yield Cu I L + activators, which establish the ATRP equilibrium in the presence of R-X initiator. <ref type="bibr">[23]</ref><ref type="bibr">[24]</ref><ref type="bibr">[25]</ref> Simultaneously, Cu I L + species can coordinate O 2 dissolved in the system, generating Cu I X(O 2 )L + ; once photoexcited, these compounds can recombine with L, yielding oxidized species (L ox ) while regenerating Cu I L + activators. <ref type="bibr">[26]</ref><ref type="bibr">[27]</ref><ref type="bibr">[28]</ref> Within a closed or highly confined reaction setup that has not been deoxygenated (i.e., with a limited amount of dissolved oxygen), this process continues until all O 2 has been consumed. Oxygen consumption is mirrored by a certain induction time before steady polymer growth can be attained, whereas during SI-photoATRP within confined setups&#65533;such as in the case of surfaces covered by a transparent glass substrate <ref type="bibr">21</ref> &#65533;continuous diffusion of oxygen from the open sides of the polymerization setup leads to inhibition of polymer brush growth at the "edges" of the substrate.</p><p>Hence, SI-photoATRP shows effective tolerance toward nondeoxygenated reaction mixtures just when highly confined polymerization setups are employed, i.e., when oxygen diffusion toward the propagating brush interface is significantly hindered. <ref type="bibr">4,</ref><ref type="bibr">11,</ref><ref type="bibr">21,</ref><ref type="bibr">22</ref> Both the confinement and "edge effect" can be alleviated upon introducing an untethered ATRP initiator, resulting in the generation of radicals that quickly recombine with adventitious oxygen, limiting its detrimental effect on the polymerization. <ref type="bibr">4</ref> Nevertheless, the scalable fabrication of polymer brushes from diverse materials requires the development of fully open-air polymerization procedures, which are effective within industrially relevant settings, i.e., without the application of confined polymerization setups. <ref type="bibr">3,</ref><ref type="bibr">5</ref> It was recently demonstrated that a fully oxygen-tolerant photoATRP can be attained by exploiting low-energy red/ NIR-light irradiation in the presence of methylene blue (MB + ) acting as a cocatalyst and dimethyl sulfoxide (DMSO), providing the controlled growth of chemically diverse polymers under open-air conditions. <ref type="bibr">29,</ref><ref type="bibr">30</ref> The mechanism of red-light-driven photoATRP involves a reductive quenching cycle whereby the excitation of MB + generates the triplet-state 3 MB + *, which is reduced by an electron donor to MB &#8226; (Figure <ref type="figure">1</ref>). The latter reduces Cu II deactivators by single electron transfer, generating Cu I L + species and simultaneously reforming ground-state MB + . <ref type="bibr">29</ref> Effective consumption of O 2 in the polymerization mixture is predominantly enabled through the reaction of 3 O 2 with 3 MB + *, which forms singlet oxygen that reacts with DMSO to yield the corresponding sulfone (Figure <ref type="figure">1</ref>).</p><p>The unprecedented tolerance of red-light-driven photo-ATRP toward environmental conditions makes it the ideal process for the fabrication of polymer brushes under technologically relevant settings. Red light features a high penetration depth within organic materials, enabling SI-photoATRP from three-dimensional (3D) supports and porous substrates. In addition, both red light and MB + are biocompatible and harmless toward biological samples, potentially making red light-driven photoATRP an ideal tool for functionalizing morphologically different biomaterials.</p><p>Inspired by the attractive traits of the corresponding solution process, here we investigated the main features of red lightdriven SI-photoATRP. We particularly focused on a catalytic system based on Cu/TPMA-MB + , which was activated through red-light irradiation at &#955; max = 625 nm. The influence on brush growth by polymerization mixture composition, light intensity, and wavelength was systematically investigated. Optimization of grafting conditions enabled the fast growth of compositionally different brushes under completely open-air conditions, both from flat, macroscopic surfaces and from porous materials (Figure <ref type="figure">1</ref>).</p><p>Especially within a microporous 3D material, we demonstrated that varying the wavelength of light that triggers ATRP equilibrium enables polymer grafting at different depths, alternatively stimulating brush growth just in its outer volume or uniformly across the support.</p><p>Red light-driven SI-photoATRP thus demonstrates an extremely versatile technique for generating brush coatings on a variety of substrates under open-air conditions, circumventing the requirements characterizing other oxygen-tolerant SI-RDRP methods.</p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head n="2.">EXPERIMENTAL SECTION</head></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head n="2.1.">Functionalization of the SiO</head><p>x Substrate with an ATRP Initiator Layer. Silicon substrates were cut (1 cm &#215; 2 cm) and cleaned with piranha solution (3:1 mixture (v/v) of H 2 SO 4 and H 2 O 2 ) for 1 h. Then, they were rinsed with ultrapure water and ethanol and dried under a stream of N 2 . The cleaned substrates were placed in a desiccator and functionalized with (3-aminopropyl)triethoxysilane (APTES) by vapor deposition under vacuum. After 3 h, the functionalized substrates were washed with ultrapure water, ethanol, and toluene and then dried under a stream of N 2 . &#945;-Bromoisobutyryl bromide (BiBB, 0.2 mL), triethylamine (TEA, 0.2 mL), and dry dichloromethane (DCM, 20 mL) were added to an Erlenmeyer flask containing the APTES-bearing substrates and let react for 2 h. Subsequently, the ATRP initiator-functionalized substrates were washed with DCM and ethanol and dried under N 2 .</p><p>2.2. Typical Procedure for the Preparation of the Polymerization Mixture. First, the following stock solutions were prepared: (i) 50 mM CuBr 2 , 300 mM TPMA, or Me 6 TREN in DMSO, and (ii) 25 mM MB + in ultrapure water. A representative polymerization mixture was then prepared by mixing ultrapure water (3.45 mL), oligo(ethylene glycol)methyl ether methacrylate M n &#8764; 500 Da (OEGMA, 1 mL), DMSO (400 &#956;L), an aliquot of the Cu complex stock solution (100 &#956;L), and of the MB + stock solution (50 &#956;L). For some experiments, stock solutions of NaX (200 mM in milli-Q) and ethyl &#945;-bromoisobutyrate (EBiB, 50 mM in DMSO) were prepared and added to the polymerization mixture as needed.</p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head n="2.3.">SI-PhotoATRP under</head><p>Confinement. An initiator-functionalized substrate was placed on a glass Petri dish and covered with 1 &#956;L cm -2 of a polymerization mixture and a glass slide. Then, the red-light (&#955; max = 625 nm) source (CHROLIS C1 LED light source, Thorlabs) was turned on. The light source was placed at a distance of 15.5 cm from the substrate, and the light intensity measured on the substrate with a power meter (Thorlabs) was 4 mW cm -2 . The intensity was varied by changing the distance of the light source from the substrate. After the desired polymerization time, the light was turned off, and the substrates were washed with ethanol and ultrapure water and dried under a stream of N 2 .</p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head n="2.4.">SI-PhotoATRP in Open</head><p>Air. An initiator-functionalized substrate was placed on a glass Petri dish (with a diameter of 5.7 cm), which was filled with 5 mL of polymerization mixture uniformly covering the substrate. For some experiments, a smaller Petri dish (diameter of 2.9 cm) was employed to reduce the total reaction volume. The red-light source was positioned above the Petri dish at a distance of 25.5 cm to obtain a light intensity on the substrate of 4 mW cm -2 . For SI-photoATRP under different light wavelengths, the same light source was employed and set to the desired wavelength (UV: &#955; max = 365 nm, blue: &#955; max = 420 nm, green/yellow: &#955; max = 565 nm, NIR: &#955; max = 780 nm). The distance of the source from the substrate was regulated to keep the light intensity on top of the substrate constant at 4 mW cm -2 . After polymerization, the light was turned off, and the substrates were thoroughly washed with ultrapure water and ethanol, followed by drying under a stream of N 2 .</p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head n="2.5.">SI-PhotoATRP under Red Light in a Deoxygenated</head><p>Environment. An initiator-functionalized substrate was placed vertically in a glass vial using Teflon spacers as a support. 3.5 mL of the polymerization mixture was added to the vial to cover the substrate, and it was degassed with Ar for 30 min. Then, the substrate was irradiated under the red-light source at a distance of 25.5 cm (light intensity of 4 mW cm -2 ). After the desired polymerization time, the light was turned off, and the vial stopper was removed. The substrate was washed with ultrapure water and ethanol and dried under a stream of N 2 .</p><p>2.6. Chitosan Cryogels Preparation and Functionalization with Polymer Brushes. Chitosan (CS) cryogels were synthesized following a reported procedure. <ref type="bibr">31</ref> First, 300 mg of CS was uniformly dispersed in 10 mL of ultrapure water. Then, 200 &#956;L of acetic acid was added, and the mixture was stirred for 5 h at 40 &#176;C. The resulting solution was transferred to a reaction mold and freeze-dried overnight to form a scaffold. Finally, the scaffold was immersed in a 2 M NaOH solution for 6 h to promote the cross-linking process.</p><p>The obtained CS cryogel was submerged in a solution composed of 10 mL of tetrahydrofuran (THF), 0.5 g of 4-dimethylaminopyridine (DMAP), and 0.5 mL of TEA. The solution was degassed with Ar for 30 min. Subsequently, 0.5 mL of BiBB in 10 mL of THF was added dropwise while the flask was maintained in an ice bath. After BiBB was added, the ice bath was removed, and the solution was stirred at room temperature for 24 h.</p><p>The ATRP initiator-functionalized CS cryogel was soaked with 0.4 mL of polymerization mixture comprising either OEGMA or 3sulfopropyl methacrylate (SPMA) as the monomer (20 vol %, with 60 vol % water and 20 vol % DMSO), and irradiated for 4 h under either red or UV light (&#955; max = 625 or 365 nm, respectively). After polymerization, the cryogel was thoroughly rinsed with ultrapure water and ethanol and freeze-dried.</p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head n="2.7.">SI-PhotoATRP in Open Air from Stainless Steel Objects.</head><p>Stainless steel objects were cleaned and functionalized with ATRP initiators using similar protocols to those for SiO x substrates (Section 2.1). The functionalized blade was placed on a Petri dish and covered with 5 mL of polymerization mixture. The Petri dish was placed under a red-light source at a light intensity of 4 mW cm -2 for 4 h. In the case of the spoon, the polymerization mixture was dropped inside the initiator-functionalized spoon bowl, which was irradiated with a redlight source at a light intensity of 4 mW cm -2 for 10 h. After polymerization, the objects were washed with ultrapure water and ethanol and dried under a stream of N 2 .</p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head n="3.">RESULTS AND DISCUSSION</head></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head n="3.1.">SI-PhotoATRP under Red Light in a Confined</head><p>Setup. SI-photoATRP in the presence of MB + and under redlight irradiation was initially investigated within confined environments by dispensing a nondegassed polymerization mixture (1 &#956;L cm -2 ) on ATRP initiator-functionalized SiO x substrates and subsequently covering the surface with a borosilicate glass slide (Figure <ref type="figure">2a</ref>,<ref type="figure">b</ref>). Polymerization solutions comprised OEGMA (20 vol %), H 2 O (70 vol %), DMSO (10 vol %), CuBr 2 /TPMA as the catalyst and MB + as the cocatalyst ([MB + ]/[Cu] = 0.25), and a 5-fold excess of TPMA relative to Cu to serve as the electron donor. Following 30 or 60 min of red-light irradiation (&#955; max = 625 nm) at an intensity of 35 mW cm -2 , POEGMA brushes with dry thicknesses (T dry ) of 16 &#177; 1 and 20.3 &#177; 0.4 nm, respectively, were successfully fabricated, as confirmed by variable angle spectroscopic ellipsometry (VASE) (Figures <ref type="figure">2c in S1</ref>). When irradiation was prolonged until 180 min, relatively thicker POEGMA brushes were generated, reaching T dry = 27 &#177; 2 nm. By varying the composition of the polymerization mixture, the role of each component could be highlighted. As shown in Table <ref type="table">S1</ref> (entries 1-4), both CuBr 2 and TPMA were necessary to obtain substantial brush growth. Either lower or higher concentrations of CuBr 2 resulted in thinner POEGMA brushes (i.e., lower molar mass), whereas increasing [MB + ] had no substantial effect on the film thickness (Table <ref type="table">S1</ref>, entries 5-8).</p><p>In contrast, the intensity of red light played a major role in the polymerization process. Relevantly, when the light intensity was decreased to 13 and 4 mW cm -2 , T dry increased to 22.3 &#177; 3.3 and 36.4 &#177; 5.9 nm, respectively, after 30 min of irradiation (Figure <ref type="figure">2c</ref>). An increase in light intensity was presumably mirrored by a concomitant increment in the concentration of the Cu I activator within the polymerization mixture. Hence, as it was previously observed for zerovalent metal-mediated SI-ATRP, higher concentrations of Cu I activator did not translate into faster brush growth but rather led to an increment in the occurrence of chain termination and thus a decrease in brush thickness and/or grafting density. <ref type="bibr">7,</ref><ref type="bibr">32,</ref><ref type="bibr">33</ref> Notably, a steady growth of brushes was attained by a 6-fold decrease of light intensity compared to what was previously recorded for polymerizations performed in solution (4 mW cm -2 for SI-photoATRP vs 25 mW cm -2 for photoATRP in solution). <ref type="bibr">29,</ref><ref type="bibr">30</ref> 3.2. SI-PhotoATRP under Red Light in Open Air. While growing polymer brushes within highly confined environments enables the consumption of oxygen dissolved in the mixture and thus avoids deoxygenation, the possibility of growing polymer brushes in completely open air could greatly simplify the reaction setup, in this way broadening the substrate scope and the applicability of the entire process. The addition of MB + in photoATRP introduces various routes for O 2 scavenging, as highlighted in Figure <ref type="figure">1</ref>.</p><p>These include (i) the reaction of excited 3 MB* with 3 O 2 , (ii) the oxidation of MB &#8226; , and (iii) the oxidation of Cu I species generated through the reductive quenching cycle (Figure <ref type="figure">1</ref>). <ref type="bibr">29</ref> Therefore, we attempted to grow POEGMA brushes from an ATRP initiator-functionalized SiO x substrate placed in the middle of an uncovered Petri dish (Figure <ref type="figure">3a</ref>). The Petri dish was filled with 5 mL of a reaction mixture to submerge the substrate. Upon 90 min of red-light irradiation at an intensity of 4 mW cm -2 , POEGMA brush films with a T dry = 146 &#177; 7 nm were obtained (Table <ref type="table">1</ref>, entry 1). Control experiments indicated that both MB + and CuBr 2 /TPMA were needed to ensure the growth of POEGMA brushes (Table <ref type="table">1</ref>, entries 2 and 3).  The use of 10 vol % DMSO was essential to enable SI-photoATRP to occur in an open-air setup. Indeed, no brush growth was measured in the absence of DMSO, whereas a relatively thin, highly inhomogeneous film was obtained by performing SI-photoATRP with only 2 vol % of DMSO (Figure <ref type="figure">S2</ref>). In contrast, DMSO contents higher than 10 vol % did not translate into a substantial benefit, while using the sole DMSO as solvent decreased the polymerization rate, generating brushes with T dry = 44 &#177; 3 nm after 3 h of irradiation (Table <ref type="table">S2</ref>). Under these conditions, the observed slower brush growth could be attributed to the lower polarity of DMSO relative to a mixture of water/DMSO (7/1 v/v), which reduced the equilibrium constant and the rate constant of activation of dormant species in ATRP. <ref type="bibr">34</ref> Under optimized conditions, brush growth rates measured by ex situ VASE revealed a linear increase in polymer brush thickness over time (Figure <ref type="figure">3b</ref>) with no evident induction period. This behavior suggests a controlled polymerization process 1 in which oxygen is readily scavenged and cannot hamper the radical generation and propagation processes. Relevantly, the application of a higher light intensity of 13 mW cm -2 had no substantial effect on the brush growth kinetics (Figure <ref type="figure">3b</ref> and Table <ref type="table">1</ref>, entry 4), whereas the brush films obtained under these conditions were less uniform, presumably due to chain termination reactions caused by an increase in activator contents (Figure <ref type="figure">S3</ref>).</p><p>Sequential polymerization/chain extension steps allowed us to generate brushes with high thicknesses. A first SI-photoATRP step led to POEGMA brushes with T dry of 100 &#177; 5 following 1 h of irradiation. After extensive rinsing, the substrate was placed in a newly prepared reaction mixture and irradiated for an additional 1 h, leading to a marked increase in the POEGMA brush thickness, which reached T dry = 163 &#177; 8 nm. A third polymerization step finally resulted in a T dry of 212 &#177; 14 nm. The progressive and rather linear increase in brush thickness upon sequential polymerization/chain extension stages (Figure <ref type="figure">3c</ref>) suggests that red light-mediated SI-photoATRP was well-controlled and confirms the suitability of this method for synthesizing high-molar mass brushes (i.e., significantly thick films with T dry &gt; 200 nm). <ref type="bibr">35</ref> It is important to emphasize that by applying an irradiation time t &#8805; 60 min, a non-negligible amount of polymer was generated in solution, especially concentrated near the substrate, i.e., in the proximity of the brush propagating front. For t &gt; 90 min, the polymer layer was very difficult to remove from the substrate. Sampling of the polymerization mixture after 90 min of light irradiation allowed us to estimate a monomer conversion of &#8764; 50% (as measured by 1 H NMR) in the reaction volumes nearby the substrate, whereas monomer conversion &lt;10% was recorded in the bulk solution (further away from the substrate).</p><p>A possible cause of radical generation in solution stems from the reaction of dissolved O 2 with either MB &#8226; or Cu I L + , resulting in the formation of the superoxide anion O 2</p><p>&#8226;-(Figure <ref type="figure">1</ref>). The latter can be further reduced to H 2 O 2 36,37 that reacts with Cu I L + via a Fenton-type reaction to form hydroxyl radicals, HO &#8226; , which can initiate new chains. These oxygen-scavenging pathways were generally negligible for similar photoATRP systems in solution; however, their contribution became more pronounced upon decreasing the concentration of ATRP initiator below 0.3 mM (i.e., targeting a degree of polymerization of 1000 or higher). <ref type="bibr">29</ref> Considering that in SI-photoATRP, the concentration of surface-bound initiator is extremely small (as it is in the case of any surface-confined ATRP process), it is plausible that the generation of O 2</p><p>&#8226;-and the consequent formation of propagating radicals in solution cannot be neglected.</p><p>While these radicals can cause polymerization to occur in solution, they can also contribute to shifting the ATRP equilibrium to the Cu I activator, thus accelerating surface polymerization. This phenomenon could contribute to the higher film thickness obtained in open air in comparison to the confined system under similar reaction conditions (i.e., T dry = 42 &#177; 10 nm vs 146 &#177; 7 nm upon 90 min of reaction with redlight irradiation at 4 mW cm -2 , Figures <ref type="figure">2c</ref> and <ref type="figure">3b</ref>, respectively).</p><p>It is also relevant to highlight that a similar SI-photoATRP process performed within a sealed vial by employing 3.5 mL of carefully deoxygenated polymerization mixture resulted in POEGMA brushes with T dry = 113 &#177; 1 nm after 90 min (i.e., &#8764; 20% lower thickness compared to that obtained through an open air process) with no signs of polymer formed in solution. This further indicates that O 2 plays a role in radical generation in solution.</p><p>We attempted to facilitate the removal of unbound polymer from the substrate by limiting its molecular weight through the addition of an untethered ATRP initiator, EBiB, to the polymerization mixture. Simultaneously, EBiB can enhance O 2 consumption by generating radicals that can recombine with oxygen. However, the polymerization from the surface became progressively slower with an increase in [EBiB] (Table <ref type="table">S3</ref>). The observed slower polymer brush growth can be attributed to the accumulation of Cu II -based deactivators, caused by the termination of radical species generated in solution from EBiB upon reaction with O 2 and derived species. <ref type="bibr">4</ref> Additionally, size exclusion chromatography (SEC) analysis of the polymerization mixture collected after 90 min of SI-photoATRP in the presence of 0.1 mM EBiB showed a polymer with M n values of &#8764; 135 kDa and D&#821; values of &#8764; 2.8 (Figure <ref type="figure">S4</ref>). Since a polymer layer concentrated on top of the substrate was visible, we attempted to analyze this unbound polymer by GPC, which revealed an M n of &#8764; 174 kDa and a very broad molecular weight distribution (D&#821; &#8764; 14, Figure <ref type="figure">S4</ref>). Thus, radical generation and uncontrolled propagation still occur in the presence of a free initiator.</p><p>Nevertheless, it must be noted that no polymer in solution could be visually detected when investigating monomers different from those of the OEGMA (vide inf ra). In addition, the extent of polymerization in solution was dependent on the height of the solution film above the substrate and on the ratio of substrate area to reaction volume (S/V). When the S/V was increased from 0.4 to 1.6 cm -1 (Table <ref type="table">S4</ref>), the substrate could be easily cleaned after 90 min of polymerization, which returned a brush thickness of 107.9 &#177; 2.0. We hypothesized that a substantial increase in S/V would reduce the exchange surface available for the O 2 molecules, mitigating its impact on the reactions. The increase in S/V was obtained by reducing both the size of the Petri dish and the reaction volume. These parameters influenced not only the extent of solution polymerization but also the brush thickness (Table <ref type="table">S4</ref>). Indeed, thicker polymer brush films were obtained upon reduction of the height of the liquid mixture covering the substrate. Various factors can contribute to this trend, including O 2 diffusion and light penetration through the polymerization mixture. We can thus conclude that the optimal setup for growing brushes in open-air systems features (i) high S/V and (ii) the lowest amount of polymerization mixture that offers a uniform coverage of the substrate.</p><p>Finally, the effect of halide salts on red-light-mediated SI-photoATRP in open air and S/V = 0.4 cm -1 was investigated. Aqueous ATRP systems are characterized by high values of the ATRP equilibrium and activation rate constants, K ATRP and k act , respectively, and low stability of the deactivator X-Cu II L + , which tends to dissociate into X -and Cu II L 2+ (which cannot deactivate propagating radicals). <ref type="bibr">38,</ref><ref type="bibr">39</ref> Hence, a large excess of halide ions relative to the Cu catalyst is generally introduced to increase the deactivation efficiency and promote control over the polymer growth. For aqueous SI-ATRP, controlled brush growth has been reported both in the absence and presence of halide salts. <ref type="bibr">[40]</ref><ref type="bibr">[41]</ref><ref type="bibr">[42]</ref><ref type="bibr">[43]</ref><ref type="bibr">[44]</ref><ref type="bibr">[45]</ref> The addition of NaBr or NaCl to open air SI-photoATRP caused a decrease in the POEGMA brush growth rate (Figure <ref type="figure">3b</ref> and Table <ref type="table">S5</ref>), with average film thickness decreasing with increasing [NaX]. For [NaX] = 5 mM, T dry = 40 &#177; 4 and 93 &#177; 4 nm were measured for X = Cl and X = Br, respectively, after 90 min of irradiation. This result indicated that the addition of NaX improved deactivator stability&#65533;with Cl -binding more strongly to Cu II complexes than Br 39 &#65533;and promoted deactivation efficiency, consequently slowing polymer brush growth.</p><p>Simultaneously, the introduction of NaX sensibly decreased the extent of polymer formation in solution. In the case of reaction mixtures comprising [NaBr] = 2 mM polymerization/ irradiation time could be extended to 150 min while avoiding the formation of a significant amount of polymer in solution and obtaining POEGMA brushes with T dry = 178 &#177; 20 nm. Under these conditions, the increase in brush thickness remained linear over time; however, a short induction period of &#8764; 15 min was recorded. This could be attributed to the increased concentration of effective deactivator, which determined a longer irradiation time necessary to generate a sufficient amount of Cu I activating species.</p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head n="3.3.">Monomer Scope and Irradiation Wavelengths.</head><p>The monomer scope for red light-mediated SI-photoATRP in open air was tested employing different water-soluble monomers (Table <ref type="table">2</ref>). Polymer brushes were effectively grown using neutral, zwitterionic, and negatively charged methacrylate monomers (Figure <ref type="figure">S5</ref>), including OEGMA of various OEG side-chain lengths, 2-methacryloyloxyethyl phosphorylcholine (MPC), 2-(N-3-sulfopropyl-N,Ndimethylammonium)ethyl methacrylate (DMAPS), and 3sulfopropyl methacrylate (SPMA). The polymerization of oligo(ethylene glycol)methyl ether acrylate (OEGA) was markedly slower than that of the corresponding methacrylate monomers, even by employing a more active ATRP catalyst, i.e., Cu/tris [2-(dimethylamino)ethyl]amine (Me 6 TREN). In contrast, poly(N-isopropylacrylamide) (PNIPAM) brushes were grown more rapidly by employing Cu/Me 6 TREN than with Cu/TPMA, reaching T dry = 89 &#177; 8 and 3 &#177; 1 nm, respectively, after 90 min of irradiation.</p><p>Additionally, MB + has a rather broad absorption spectrum (Figure <ref type="figure">4</ref>); thus, the Cu/L-MB + dual catalytic system could be used to catalyze photoATRP under irradiation at different light wavelengths. <ref type="bibr">29</ref> POEGMA brush films with T dry &#8764; 95 nm (Figure <ref type="figure">4</ref> and Table <ref type="table">S6</ref>) were obtained upon 90 min exposure to either UV or green/yellow light (&#955; max = 365 and 565 nm, respectively, at an intensity of 4 mW cm -2 ). In contrast, no brush growth was observed by subjecting the polymerization setup to blue (&#955; max = 420 nm) and NIR (&#955; max = 780 nm) light irradiation at the same intensity due to the minimal absorbance of MB + in these spectral regions (Figure <ref type="figure">4</ref>).</p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head n="3.4.">SI-PhotoATRP from 3D</head><p>Substrates. An important advantage of low-energy light over shorter wavelengths is represented by its enhanced penetration through non-transparent materials. For instance, Hawker, Boyer et al. exploited a NIR light-mediated SI-PET-RAFT polymerization to grow polymer brushes within the inner walls of opaque silicone tubes. <ref type="bibr">12</ref> Thus, the enhanced penetration offered by the red light-mediated SI-photoATRP could enable the growth of polymer brushes within porous substrates, uniformly decorating not only the external walls but also the interior of pores, cavities, and channels. To demonstrate this, the Cu/L-MB + catalytic system was employed to functionalize a CS-based cryogel (Figures <ref type="figure">1</ref> and <ref type="figure">S6</ref>) in open air. 3D substrates based on CS are technologically relevant supports for polymer brush modification, as they have been frequently employed as tissue engineering constructs and, more generally, as biocompatible biomaterial platforms. <ref type="bibr">31,</ref><ref type="bibr">46,</ref><ref type="bibr">47</ref>    CS cryogels were reacted with BiBB to introduce C-Br groups that served as initiating sites for the subsequent SI-photoATRP. The modified supports were later soaked in a polymerization mixture comprising MB + , CuBr 2 /TPMA, and SPMA or OEGMA as monomer in water with 10 vol % DMSO. Soaked supports were irradiated for 90 min with red light. After extensive washing, the 3D supports were sectioned and analyzed by attenuated total reflectance infrared spectroscopy (ATR-IR) and scanning electron microscopy coupled with energy-dispersive X-ray spectroscopy (SEM-EDS) in order to characterize the composition of both the inner volumes and the outer part of the porous structure (Figure <ref type="figure">5a-c</ref>). Following red-light irradiation, a uniform growth of polymer brushes was recorded across the entire CS structure in the case of both PSPMA and POEGMA (Figures <ref type="figure">5b</ref>, <ref type="figure">S7a</ref>, and <ref type="figure">S8</ref>). When a similar grafting process was repeated on a new set of initiator-functionalized supports under UV light irradiation (&#955; max = 365 nm, 4 mW cm -2 ), the growth of brushes was evidently more marked on the external volumes of the gel structure, while ATR-IR recorded little or no evidence of polymer grafts within the inner section of the cryogels (Figures 5c, S7b Finally, to demonstrate the versatility of red-light-mediated SI-photoATRP, we focused on functionalizing objects with varying shapes and surface curvatures, such as a stainless-steel blade and a spoon (Figure <ref type="figure">5d</ref>,<ref type="figure">e</ref>). ATRP initiators were deposited on the surfaces of these objects using an approach similar to that employed for SiO 2 substrates. The blade was placed in a Petri dish, similar to the flat SiO 2 substrates, covered with the standard polymerization mixture, and irradiated with red light for 4 h. To grow brushes from the curved surface of the spoon, the polymerization mixture was poured directly into the spoon, which was then irradiated with red light from above. After thorough washing, both objects showed visibly less reflective surfaces, and the change in color reflected the presence of a uniform and relatively thick brush coating.</p><p>Red light-driven SI-photoATRP in open air gives access to growing polymer brushes at scale from materials with diverse shapes, overcoming the limitations imposed by confined setups and facilitating the implementation of SI-ATRP in realistic settings.</p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head n="4.">CONCLUSIONS</head><p>The combination of MB + -and Cu-based ATRP catalyst enables red light-driven SI-photoATRP under fully open-air conditions, addressing long-standing limitations related to oxygen sensitivity and confinement requirements in traditional SI-ATRP methods. Rapid growth of polymer brushes with tunable dry thickness was achieved from flat substrates, using different monomers and water as the solvent, with a small fraction of DMSO that contributes to scavenging oxygen.</p><p>The high penetration depth of red light within organic materials was exploited to uniformly grow polymer brushes from 3D microporous supports. Additionally, the possibility of activating the MB + -Cu/L catalytic system with different irradiation wavelengths enabled the selective growth of brushes from the support in different positions, i.e., throughout its entire structure (using red light) or mainly at its outer surface (exploiting UV light).</p><p>Finally, this approach enabled the growth of brushes on objects with complex geometries, including curved and irregular surfaces, demonstrating versatility and scalability that are unattainable with traditional SI-ATRP systems.</p><p>Red light-mediated SI-photoATRP emerges as a robust, fully oxygen-tolerant process that can be translated into relevant industrial and biomedical settings, where process simplicity, material diversity, and scalability are essential.</p></div>
<div xmlns="http://www.tei-c.org/ns/1.0"><head>&#9632; ASSOCIATED CONTENT</head></div><note xmlns="http://www.tei-c.org/ns/1.0" place="foot" xml:id="foot_0"><p>https://doi.org/10.1021/acsami.5c08584 ACS Appl. Mater. Interfaces 2025, 17, 38773-38782</p></note>
			<note xmlns="http://www.tei-c.org/ns/1.0" place="foot" xml:id="foot_1"><p>https://doi.org/10.1021/acsami.5c08584</p></note>
		</body>
		</text>
</TEI>